“Since the observed amount of slip cannot be attributed to high kinetic energy of moving dislocations, it is necessary to postulate a dislocation multiplication process… requiring only small dislocation velocities.”F. C. Frank & W. T. Read · Physical Review 79, 722 (1950)
Every gliding dislocation exits the crystal surface as a slip step and vanishes forever—yet cold working drives dislocation density from \(10^{10}\text{ m}^{-2}\) in annealed metals up to \(10^{16}\text{ m}^{-2}\). Where do all the new dislocations come from?
Why does an fcc \(\frac{a}{2}[\bar{1}10]\) perfect dislocation split into two partials across a higher-energy stacking fault—and why do screws cross-slip effortlessly in pure Al yet stay locked onto planar arrays in 304 stainless steel?
With \(48\) slip systems in bcc iron, why does its yield stress surge in winter to trigger brittle cleavage? And why does fcc Cu deep-draw easily at room temperature while close-packed hcp Mg cracks during cold rolling?
Our five-step arc tracks conservative glide & Peierls stress \(\to\) climb, cross-slip & Frank–Read sources \(\to\) Shockley partials, Frank loops & Thompson locks \(\to\) bcc screw cores & hcp twinning.
d/b = 0.82
T = 120 K
| Feature | fcc (Cu, Al, Ni, \(\gamma\)-Fe) | bcc (\(\alpha\)-Fe, W, Mo, Cr) | hcp (Mg, Zn, Ti, Zr) |
|---|---|---|---|
| Shortest Perfect \(\boldsymbol{b}\) | \(\frac{a}{2}\langle 110\rangle\) (\(|\boldsymbol{b}|=\frac{\sqrt{2}}{2}a\)) | \(\frac{a}{2}\langle 111\rangle\) (\(|\boldsymbol{b}|=\frac{\sqrt{3}}{2}a\)) | \(\frac{1}{3}\langle 11\bar{2}0\rangle\) (\(\langle a\rangle\)) & \(\frac{1}{3}\langle 11\bar{2}3\rangle\) |
| Primary Slip Systems | \(\{111\}\langle 110\rangle\) (\(12\) total, \(5\) indep.) | \(\{110\}/\{112\}/\{123\}\langle 111\rangle\) (\(48\)) | Mg basal \((0001)\); Ti/Zr prism \(\{10\bar{1}0\}\) |
| Dislocation Core | Planar \(\{111\}\) split into two Shockley partials + fault | Threefold non-planar screw core (no stable fault) | Controlled by \(c/a\) and basal vs. prism \(\gamma_{\mathrm{SF}}\) |
| Peierls Stress & \(T\)-Sensitivity | Minimal; \(\sigma_y\) nearly flat down to \(4\text{ K}\) | High (kink-pair activated); \(\sigma_y\) surges at low \(T\) | Low on basal/prism; very high for pyramidal \(\langle c+a\rangle\) |
| Cross-Slip & Slip Traces | Set by \(\gamma_{\mathrm{SF}}\) (Al wavy; 304 SS planar) | Frequent screw plane-switching (wavy pencil glide) | Restricted; accompanied by twinning & strong texture |
| Cryogenic Toughness | No DBTT (ideal for LNG / \(\mathrm{LH_2}\) cryotanks) | Pronounced DBTT (winter cleavage risk) | Mg/Zn cold-brittle; high-purity Ti stays tough |
Bowing past the semicircular instability \(\tau_{\mathrm{FR}}=Gb/L\) repeatedly emits loops while Koehler double cross-slip breeds new sources, multiplying \(\rho\) by \(10^6\times\); fcc zig-zag Shockley dissociation cuts \(b^2\) by \(33.3\%\), with high-\(\gamma_{\mathrm{SF}}\) \(\mathrm{Al}\) constricting easily to cross-slip and low-\(\gamma_{\mathrm{SF}}\) 304 SS locked into planar slip.
bcc \(\frac{a}{2}\langle 111\rangle\) screws have threefold non-planar cores whose thermally activated kink-pairs freeze in winter cold to trigger cleavage (DBTT); hcp \(\langle a\rangle\) slip lacks \(c\)-axis strain and \(5\) independent systems, requiring \(\langle c+a\rangle\) slip or twinning.
Next Lecture (From Single Dislocations to Bulk Yielding & Strengthening) — Dislocations, Plasticity & Recrystallization III: Schmid's law, Taylor factor, work hardening & Considère necking, Cottrell atmospheres & Lüders bands, and the four strengthening mechanisms.
1. Given \(G=80\text{ GPa}\), \(b=0.25\text{ nm}\), and pin spacing \(L=100\text{ nm}\), what is the Frank–Read critical stress \(\tau_{\mathrm{FR}}\), and how do climb and cross-slip differ?
From \(\tau_{\mathrm{FR}}=Gb/L\), \(80\text{ GPa}\times 0.25\text{ nm}/100\text{ nm}=200\text{ MPa}\); edge climb is vacancy-mediated, whereas pure screw cross-slip is conservative.
2. In fcc crystals, regarding \(\frac{a}{2}[\bar{1}10]\to\frac{a}{6}[\bar{2}11]+\frac{a}{6}[\bar{1}2\bar{1}]\) and the Thompson reaction \(\boldsymbol{\delta A}+\boldsymbol{A\beta}\to\boldsymbol{\delta\beta}\), which statement is true?
Width \(d\propto 1/\gamma_{\mathrm{SF}}\), so low \(\gamma_{\mathrm{SF}}\) widens ribbons and resists constriction; fusing two Shockleys drops \(b^2\) from \(12\) to \(2\) (\(a^2/36\)) into a sessile stair-rod.
3. Comparing dislocation behavior in bcc iron versus hcp titanium and magnesium, which statement is completely accurate?
bcc screws have non-planar threefold cores requiring thermal kink-pairs (driving DBTT); Ti/Zr favor prism slip, and basal \(\langle a\rangle\) gives only \(2\) independent systems.