FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 13 (CAPSTONE)

Fracture & Failure of Materials II

Micro-Mechanisms, Forensic Fractography, DBTT Competition & Fatigue Life
CLEAVAGE, DIMPLES, DBTT COMPETITION & PARIS FATIGUE LIFE · PART 2
“Every fracture surface is a crime-scene transcript left by the crack: river patterns trace cleavage back to its origin, dimples record plastic dissipation, and each fatigue striation counts a single load cycle.”Fundamentals of Materials Science · Ch. 13 · In Tribute to Paul C. Paris (1930–2017)
Liang Wumse3d.com · Smart Classroom
Top: yield resistance \(\sigma_{\mathrm{ys}}(T)\) vs. cleavage stress \(\sigma_f\) sets DBTT · Bottom: fatigue beach marks & Paris crack advance
→Space NextO OverviewP PenL LaserT ThemeF Full
PROLOGUE · FROM MICRON-SCALE FRACTOGRAPHY TO THE MILLION-CYCLE SILENT KILLER

How Do Fracture Surfaces Trace Crack Origins, Why Did Titanic Shatter, and Why Do Shafts Snap Below Half Yield?

QUESTION 01 · FORENSIC FRACTOGRAPHY

How Do Surfaces Reveal Load & Origin?

A running crack leaves distinct microscopic fingerprints—cleavage river patterns, equiaxed/shear/tear dimples, rock-candy facets, and chevron marks. How do forensic investigators trace them back to the primary initiation site?

QUESTION 02 · COLD EMBRITTLEMENT

Why Does Cu Survive Liquid He While Steel Ships Shatter?

Austenitic stainless steel and pure \(\mathrm{Cu}\) stay ductile in \(-269\,^\circ\mathrm{C}\) liquid \(\mathrm{He}\), yet Titanic's carbon-steel hull fractured like glass in \(-2\,^\circ\mathrm{C}\) water—and why does grain refinement alone boost strength while lowering DBTT?

QUESTION 03 · SUDDEN FATIGUE

Why Do \(50\%\text{–}90\%\) of Failures Strike Without Warning?

Even at stress amplitudes below half of \(\sigma_{\mathrm{ys}}\), smooth crankshafts and Aloha Flight 243's fuselage tore apart after tens of thousands of cycles—how does a smooth surface nucleate microcracks, and how do we calculate safe NDT intervals?

We follow one continuous investigative chain: Cottrell cleavage vs. microvoid dimples \(\to\) Weibull statistics & fractography \(\to\) bcc DBTT competition \(\to\) S–N, Goodman & Paris fatigue life.

§ 13.2.2 – § 13.4 · Micro-Fracture, DBTT & Fatigue
LECTURE STRUCTURE · § 13.2.2 – § 13.4

Decode the Crack-Tip Cleavage-vs.-Slip Competition, Then Master the Cyclic Crack Clock via \(\Delta K\)

  1. Cleavage & DimplesCottrell \(a[001]\) wedge nucleus
    3 dimple mating-face rules
    § 13.2.2–13.2.3
  2. IG & FractographyGibbs rock-candy IG · Weibull \(m\)
    Cup-cone, chevrons & rivers
    § 13.2.4–13.2.5
  3. DBTT CompetitionCharpy S-curve · bcc double-kink
    \(k_f\gt k_y\) grain effect · irradiation
    § 13.3 · Model
  4. S–N & GoodmanBasquin vs. Manson–Coffin
    Endurance \(\sigma_e\) & mean stress
    § 13.4.1–13.4.2
  5. PSBs & Paris LawPSB extrusions & striations
    \(\mathrm{d}a/\mathrm{d}N=C(\Delta K)^m\) · Aloha 243
    § 13.4.3–13.4.5 · Model
§ 13.2.2 – § 13.4 · Fractography, DBTT & Fatigue Chain
01
PART I · § 13.2.2 – § 13.2.5

Cleavage, Microvoid Coalescence, Weibull Statistics & Fractography

Inside the micron-scale arena ahead of a crack tip: does it unzip low-index planes into river patterns, or nucleate and neck second-phase microvoids into dimples?
  1. Crystallographic cleavage planes & Cottrell \(a[001]\) dislocation-wedge nucleation05
  2. Microvoid coalescence (MVC) 3 stages & equiaxed / shear / tear dimple mating faces06
  3. Intergranular “rock-candy” embrittlement & ceramic weakest-link Weibull statistics07
  4. Forensic fractography: cup-and-cone 3 zones, chevrons, river confluence & SEM guide08
§ 13.2.2 · CLEAVAGE CRYSTALLOGRAPHY & COTTRELL (1958) DISLOCATION-REACTION NUCLEATION

Intersecting bcc Slip Dislocations React into \(a[001]\), Dropping Energy by \(1/3\) to Wedge Open \((001)\)

Characteristic Cleavage Planes Across Crystals

  • Low-index planes preferred: wide interplanar spacing \(d_{hkl}\), fewer cross-plane bonds, low surface energy \(\gamma\) — bcc metals (\(\alpha\text{-Fe, Cr, W, Mo}\)) cleave on \(\{001\}\); hcp (\(\mathrm{Zn, Mg}\)) on basal \(\{0001\}\); \(\mathrm{NaCl}\) & mica on \(\{001\}\); \(\mathrm{Al_2O_3}\) on rhombohedral \(\{1\bar{1}02\}\).
  • fcc metals resist cleavage: \(\mathrm{Cu, Al, Au, Ni}\) offer 12 close-packed slip systems with planar cores that blunt crack tips even near \(0\text{ K}\) (whereas bainite & tempered martensite exhibit quasi-cleavage facets + tear ridges).

Cottrell Cleavage-Crack Nucleation (Eq. 13.25, Fig. 13.6)

\(\begin{gathered}\frac{a}{2}[\bar{1}\bar{1}1]_{(101)}+\frac{a}{2}[111]_{(\bar{1}01)}\longrightarrow a[001]_{(001)}\\ \sum b_{\mathrm{before}}^2=\frac{3}{4}a^2+\frac{3}{4}a^2=\frac{3}{2}a^2\;\gt\;b_{\mathrm{after}}^2=a^2\;(\text{spontaneous by Frank's rule})\end{gathered}\)
  • Three laws from one reaction: ① Sessile \(a[001]\perp(001)\) acts as an atomic wedge splitting \((001)\) (in fcc, two \(\tfrac{a}{2}\langle 110\rangle\to a\langle 001\rangle\) gives \(b^2=a^2\to a^2\), zero driving force); ② coarser grains build longer pile-ups, aiding cleavage; ③ frozen low-\(T\) slip lets cleavage race at \(0.3\text{–}0.5\,c_s\).
§ 13.2.2 · Cleavage Planes, Quasi-Cleavage & Cottrell Model
§ 13.2.3 · MICROVOID COALESCENCE (MVC) & STRESS-STATE INVERSION FROM MATING DIMPLES

Particles Debond into Voids, Triaxial Tension Grows Them, and Mating Dimples Distinguish Shear vs. Tear

  • Three-stage MVC (Fig. 13.7): ① Nucleation: weak inclusions (\(\mathrm{MnS}\)) debond early, while fine bonded carbides crack/debond at \(\varepsilon\sim 0.5\text{–}1.0\); ② Growth: accelerates exponentially with hydrostatic triaxiality; ③ Coalescence: inter-void ligaments link via internal necking or shear localization.
  • Answer to Q1a (Fig. 13.8 dimple rules): tensile overload leaves equiaxed dimples; shear and tear both elongate into parabolas, resolved by comparing flipped mating faces—shear dimples point opposite on the two faces, whereas tear dimples open the same way (closed tips point back to the crack origin).
§ 13.2.3 · Microvoid Coalescence & Mating Dimple Rules
§ 13.2.4 & EXTENDED READING · INTERGRANULAR “ROCK-CANDY” FRACTURE & WEIBULL STATISTICS

Impurity Segregation Turns Grain Boundaries Brittle; Ceramic Scatter Demands \(P_f\lt 10^{-6}\) Design

\(\begin{gathered}\text{IG separation work: }W_{\mathrm{ig}}=2\gamma_{\mathrm{s}}-\gamma_{\mathrm{gb}}\xrightarrow{\mathrm{P,Sb,Sn,As}\text{ seg.}}\text{plummets}\\ \text{Weibull survival: }\;P_s=\exp\!\left[-\frac{V}{V_0}\!\left(\frac{\sigma}{\sigma_0}\right)^m\right]\end{gathered}\)
  • Four triggers of rock-candy IG facets (Fig. 13.9): ① \(\mathrm{P,Sb,Sn,As}\) segregation at \(375\text{–}575\,^\circ\mathrm{C}\) (temper embrittlement); ② continuous brittle boundary carbides; ③ hydrogen embrittlement (HE) / liquid-metal embrittlement (LME); ④ high-\(T\) creep cavitation.
  • Weibull modulus \(m\) & volume effect: \(\mathrm{Al_2O_3}\) has \(m\sim 10\) (mean \(400\text{ MPa}\), yet \(P_f\lt 10^{-6}\) allows only \(\sim 100\text{ MPa}\)), bearing \(\mathrm{Si_3N_4}\) reaches \(m\sim 20\), metals \(m\gt 50\); larger volume \(V\) samples larger flaws and fails weaker.
§ 13.2.4 & Reading · Intergranular Fracture & Weibull Law
§ 13.2.5 · CUP-AND-CONE ZONES, CHEVRON MARKS & CLEAVAGE RIVER CONFLUENCE

Follow Plate Chevron V-Tips and Trace SEM Cleavage Tributaries Upstream to Pinpoint the Primary Origin

Macro-Fractography: Cup-Cone & Chevrons (Fig. 13.10)

  • Round-bar cup-and-cone 3 zones: dull rough central fibrous zone (slow initiation) \(\to\) radial zone (fast unstable ridges) \(\to\) outer \(45^\circ\) smooth shear lip (surface plane-stress shear); higher toughness expands fibrous & shear-lip areas.
  • Plate chevron marks: radial tear ridges converge into nested V's whose V-tips always point back to the crack origin (key clue in Liberty ship hulls).

Cleavage River-Pattern Confluence Rule (Fig. 13.11)

  • Tributaries merge downstream: crossing a twist boundary or screw dislocation splits a cleavage front onto parallel planes linked by cleavage steps; to reduce step surface energy, steps merge rather than branch during growth—downstream shows crack growth; upstream locates the origin.
Fracture Mechanism (Table 13.1)Signature SEM MorphologyPhysical Origin & Crack-Tracing Clue
Cleavage / Quasi-CleavageRiver patterns, cleavage steps, tongues / fine facets + tear ridgesLow-index plane splitting; tributaries merge into main stream along growth
Microvoid Coalescence (MVC)Dimples (equiaxed / parabolic shear or tear, particles at base)Inclusion debonding & internal necking; mating faces distinguish shear vs. tear
Intergranular / Fatigue Stage II3D “rock-candy” grain facets / parallel arched fatigue striationsBoundary segregation or HE / 1 striation = 1 load cycle (spacing \(\approx\mathrm{d}a/\mathrm{d}N\))
§ 13.2.5 · Cup-Cone, Chevrons, River Patterns & Table 13.1
02
PART II · § 13.3.1 – § 13.3.4

Charpy Impact, bcc Ductile-to-Brittle Transition (DBTT) & Irradiation

The race between athermal cleavage stress \(\sigma_f\) and thermally activated yield stress \(q\sigma_{\mathrm{ys}}(T)\) decides whether steel bends or shatters in icy seas.
  1. Charpy V-notch S-curve, crystal-structure contrast (Table 13.2) & Titanic metallurgical autopsy10
  2. Unified criterion \(q\sigma_{\mathrm{ys}}(T,\dot{\varepsilon},d)\ge\sigma_f(d)\): rate, notch, grain slope \(k_f\gt k_y\) & reactor aging11
  3. Interactive Sandbox (M12·02): real-time four-factor DBTT yield–cleavage crossover12
§ 13.3.1 – § 13.3.2 & READING · CHARPY \(A_K(T)\) S-CURVE, CRYSTAL LATTICE CONTRAST & TITANIC

bcc \(\tfrac{1}{2}\langle 111\rangle\) Screw Dislocations Glide via Double Kinks: Cold Freezes Slip and Shatters Hulls

Charpy V-Notch Impact & Lattice Contrast (Table 13.2)

  • Why “V-notch + fast pendulum”: triaxial tension suppresses yielding while high strain rate (\(\sim 10^3\text{ s}^{-1}\)) starves thermal activation, exposing worst-case brittleness. \(A_K(T)\) spans upper shelf (dimples) \(\to\) steep DBTT \(\to\) lower shelf (cleavage); design requires \(T_{\mathrm{service}}^{\min}\ge\mathrm{DBTT}+(20\text{–}40\,^\circ\mathrm{C})\).
  • Answer to Q2a (Table 13.2): fcc (\(\mathrm{Cu, Al, Ni}, \gamma\text{-Fe}\)) planar cores have tiny Peierls barriers and stay ductile at \(-269\,^\circ\mathrm{C}\); bcc (\(\alpha\text{-Fe, W, Mo}\)) non-planar screw cores freeze at low \(T\), sending \(\sigma_{\mathrm{ys}}\) up \(2\text{–}4\times\) above \(\sigma_f\).

Extended Reading: 1912 Titanic Metallurgical Autopsy

  • High-P coarse-grained hull plate: acid open-hearth steel held \(3\text{–}4\times\) modern \(\mathrm{P}\) levels, giving wreck Charpy DBTTs of \(30\text{–}70\,^\circ\mathrm{C}\). In \(-2\,^\circ\mathrm{C}\) water—over \(30\,^\circ\mathrm{C}\) below DBTT—the hull sat squarely on the brittle lower shelf.
  • Slag-laden wrought-iron rivets: bow rivets rich in brittle silicate slag popped their heads without plastic stretch under iceberg compression, unzipping hull seams (modern Grade-E hull steel mandates \(\mathrm{CVN}\ge 27\text{ J}\) at \(-40\,^\circ\mathrm{C}\)).
§ 13.3.1–13.3.2 & Reading · Charpy Curve & Titanic Analysis
§ 13.3.3 – § 13.3.4 · STRAIN RATE, NOTCH TRIAXIALITY, PETCH SLOPE \(k_f\gt k_y\) & REACTOR AGING

Unified Criterion \(q\,\sigma_{\mathrm{ys}}(T,\dot{\varepsilon},d)\ge\sigma_f(d)\): Grain Refinement Alone Wins Both Strength and Toughness

External Triple Threat: Cold, High Rate & Sharp Notch

\(\begin{gathered}\dot{\varepsilon}=\dot{\varepsilon}_0\exp\!\left[-\frac{\Delta H^\ddagger(\sigma)}{k_{\mathrm{B}}T}\right]\xrightarrow{\sigma=\sigma_f}T_{\mathrm{DBT}}=\frac{\Delta H^\ddagger(\sigma_f)}{k_{\mathrm{B}}\ln(\dot{\varepsilon}_0/\dot{\varepsilon})}\approx A+B\ln\dot{\varepsilon}\\ \text{Notch triaxiality }q\approx 2\text{–}3:\;\;q\,\sigma_{\mathrm{ys}}\ge\sigma_f\iff\sigma_{\mathrm{ys}}\ge\frac{\sigma_f}{q}\;(\mathrm{DBTT}\uparrow!)\end{gathered}\)
  • Rate–temperature equivalence: each \(10\times\) jump in \(\dot{\varepsilon}\) shrinks the denominator by \(2.3\), shifting \(T_{\mathrm{DBT}}\) upward; a smooth bar ductile at \(T_1\) can snap brittlely when notched.
  • Neutron irradiation (§ 13.3.4): fast neutrons create defect nanoclusters that pin dislocations, raising RPV DBTT by \(30\text{–}80\,^\circ\mathrm{C}\) over 40 years—requiring strict low-\(\mathrm{Cu/P}\) steel and in-core surveillance capsules.

Answer to Q2b: Petch Cleavage Slope \(k_f\gt k_y\) (Eq. 13.28)

\(\sigma_{\mathrm{ys}}=\sigma_0+k_y d^{-1/2},\quad\sigma_f=\sigma_0'+k_f d^{-1/2}\;\;(k_f\gt k_y!)\)
  • Dual grain-boundary bonus: ① high-angle boundaries deflect cleavage planes, forcing re-nucleation; ② shorter pile-ups weaken Cottrell stress concentration, so refining \(d\) lifts \(\sigma_f\) faster than \(\sigma_{\mathrm{ys}}\).
  • The sole strength–toughness win-win: for \(d\lt d^*\), the \(\sigma_f-\sigma_{\mathrm{ys}}\) margin widens, forcing \(\sigma_{\mathrm{ys}}(T)\) to much lower \(T\) before catching \(\sigma_f\) — strength rises while DBTT drops (core of TMCP HSLA steels).
§ 13.3.3–13.3.4 · Strain Rate, Notch q, Petch Law & RPV Aging
§ 13.3 · REAL-TIME CROSSOVER SANDBOX FOR YIELD \(q\sigma_{\mathrm{ys}}(T)\) VS. CLEAVAGE \(\sigma_f\)

Tune Grain Size, Notch Constraint, Strain Rate, and Irradiation to Shift DBTT and the Charpy S-Curve

  • Verify the fine-grain miracle: drag grain size \(d\) from coarse to fine—blue \(\sigma_{\mathrm{ys}}\) rises, yet orange \(\sigma_f\) rises even more (\(k_f\gt k_y\)), pushing the DBTT crossover strongly leftward (to lower \(T\)).
  • Test notches & irradiation: raise notch constraint \(q\) or irradiation hardening \(\Delta\sigma\)—effective yield climbs while \(\sigma_f\) stays flat, shifting DBTT rightward (embrittlement).
  • fcc benchmark: switch to the austenitic steel preset—flat \(\sigma_{\mathrm{ys}}(T)\) stays below \(\sigma_f\) at all temperatures, never crossing.
§ 13.3 · Davidenkov–Orowan–Cottrell DBTT Competition
03
PART III · § 13.4.1 – § 13.4.5

Metal's #1 Killer — Fatigue: S–N Curves, PSBs & Paris Law

Driving \(50\%\text{–}90\%\) of mechanical failures without macro-yield: persistent slip bands nucleate micro-notches, while the Paris power law locks in safe NDT intervals.
  1. Cyclic stress metrics, HCF Basquin vs. LCF Manson–Coffin, endurance limit \(\sigma_e\) & Goodman diagram14
  2. Three fatigue stages: PSB extrusion/intrusion initiation, striations vs. beach marks & Paris law15
  3. Interactive Sandbox (M12·04): Paris life integration, Aloha Flight 243 & three design philosophies16
§ 13.4.1 – § 13.4.2 · BASQUIN / MANSON–COFFIN LAWS, ENDURANCE LIMIT \(\sigma_e\) & GOODMAN DIAGRAM

Steels Show a Horizontal Endurance Limit \(\sigma_e\) for Infinite Life; Aluminum Demands Finite-Life Retirement

\(\begin{gathered}\sigma_a=\frac{\sigma_{\max}-\sigma_{\min}}{2},\;\;\sigma_m=\frac{\sigma_{\max}+\sigma_{\min}}{2},\;\;R=\frac{\sigma_{\min}}{\sigma_{\max}}\\ \text{HCF Basquin: }\sigma_a=\sigma_f'(2N_f)^b;\quad\text{LCF Manson–Coffin: }\frac{\Delta\varepsilon_p}{2}=\varepsilon_f'(2N_f)^c\\ \text{Goodman: }\;\sigma_a=\sigma_e\!\left(1-\frac{\sigma_m}{\sigma_{\mathrm{UTS}}}\right)\;\;(\text{Soderberg uses }\sigma_{\mathrm{ys}};\text{ Gerber uses }\sigma_m^2)\end{gathered}\)
  • HCF vs. LCF & steel vs. Al (Fig. 13.14): \(N_f\gt 10^5\) is stress-controlled—mild steels & \(\mathrm{Ti}\) alloys plateau at \(10^6\text{–}10^7\) cycles (\(\sigma_e\approx 0.4\text{–}0.5\,\sigma_{\mathrm{UTS}}\), modulo VHCF internal inclusions), whereas \(\mathrm{Al}\) alloys keep sloping down and use fatigue strength \(\sigma_e'\) at \(10^7\text{–}10^8\) cycles.
  • Mean-stress check: given \(\sigma_e=250,\;\sigma_{\mathrm{UTS}}=600,\) and \(\sigma_m=200\text{ MPa}\), Goodman gives \(\sigma_a=250(1-200/600)\approx 166.7\text{ MPa}\).
§ 13.4.1–13.4.2 · S–N Curves & Goodman Diagram
§ 13.4.3 – § 13.4.5 · WOOD PERSISTENT SLIP BANDS (PSBs), STRIATIONS VS. BEACH MARKS & PARIS LAW

PSB Intrusions Consume \(60\%\text{–}90\%\) of Life on Smooth Surfaces; Cracks Then March by \(\mathrm{d}a/\mathrm{d}N=C(\Delta K)^m\)

Answer to Q3a: Three Stages & Two Band Scales (Figs. 13.16–17)

  • Stage I Initiation (\(60\%\text{–}90\%\) of \(N_f\)): cyclic shear localizes into ladder-wall persistent slip bands (PSBs), building surface extrusions & intrusions that grow along \(45^\circ\) slip planes across a few grains.
  • Stage II Propagation (\(10\%\text{–}40\%\)): turns normal to tensile stress; in SEM, 1 fatigue striation = 1 load cycle (spacing \(\approx\mathrm{d}a/\mathrm{d}N\)), whereas macroscopic beach marks record startup/shutdown or load-block shifts (arcs center on origin).
  • Stage III Overload (\(\lt 1\%\)): remaining ligament snaps via dimples or cleavage.

Paris Law & Damage-Tolerant Life Integral (Eqs. 13.36–37)

\(\begin{gathered}\Delta K=Y\Delta\sigma\sqrt{\pi a},\quad\frac{\mathrm{d}a}{\mathrm{d}N}=C(\Delta K)^m\;\;(\text{metals }m\approx 2\text{–}4,\text{ ceramics }10\text{–}50)\\ N_f=\int_{a_0}^{a_c}\frac{\mathrm{d}a}{C(Y\Delta\sigma\sqrt{\pi a})^m}=\frac{2\left(a_0^{1-m/2}-a_c^{1-m/2}\right)}{(m-2)C\,Y^m(\Delta\sigma)^m\pi^{m/2}}\;\;(m\ne 2)\end{gathered}\)
  • Log–log sigmoidal 3 regimes (Fig. 13.18): threshold (\(\lt\Delta K_{\mathrm{th}}\), non-propagating) \(\to\) linear Paris regime \(\to\) fast fracture (\(K_{\max}\to K_{\mathrm{IC}}\)).
  • Five anti-fatigue rules: ① generous fillets; ② mirror polish to delay PSBs; ③ shot peening compressive stress (\(5\text{–}10\times\) life); ④ clean fine microstructure; ⑤ schedule NDT from \(N_f\).
§ 13.4.3–13.4.5 · PSB Initiation, Striations & Paris Law
§ 13.4.4 CASE · PARIS INTEGRAL SANDBOX, ALOHA 243 MSD & FATIGUE DESIGN EVOLUTION

Debonded Lap Joints Raised Rivet \(\Delta\sigma\) to \(100\text{ MPa}\): \(N_f\propto(\Delta\sigma)^{-4}\) Predicts \(87{,}000\) Cycles on Target

\(\begin{gathered}\text{Aloha 243 (2024-T3, }m=4,\;C=1.4\times 10^{-11},\;\Delta\sigma=100\text{):}\\ a_0=0.5\to 10\text{ mm}\implies N_f\approx 8.7\times 10^4\;\text{cycles (flew }89{,}680\text{!)}\\ \text{Vessel check (}m=3,\;C=5\times 10^{-12},\;Y=1\text{):}\;N_f\approx 2.49\times 10^6\;\text{cycles}\end{gathered}\)
  • Multi-site damage (MSD) & 3 design eras: 1954 Comet square-window crashes birthed fail-safe design; Aloha 243's link-up of collinear rivet cracks drove aging-fleet rules. Engineering spans: infinite-life (\(\sigma_a\lt\sigma_e\) steel springs), safe-life (timed Al retirement), and damage-tolerant (Paris-scheduled NDT for aircraft & nuclear).
§ 13.4.4 · Paris Life & Aloha 243 MSD
LECTURE SUMMARY

Fractography Decodes the Mechanism, \(q\sigma_{\mathrm{ys}}\) vs. \(\sigma_f\) Sets DBTT, and Paris Integration Guards Cyclic Life

Cottrell Cleavage vs. Dimples→Weibull m & Crack Tracing→bcc Double-Kink & kf > ky→S–N & Goodman Rule→PSBs & Paris Life Nf
ANSWERING QUESTIONS 1 & 2

Chevron V-tips and upstream river tributaries point straight to the crack origin, while mating parabolic dimples separate shear from tear; low-\(T\) freezing of bcc screw double kinks embrittles hull steels, and only grain refinement (\(k_f\gt k_y\)) raises strength while lowering DBTT.

ANSWERING QUESTION 3

Cyclic shear builds PSB surface intrusions that nucleate cracks on smooth parts before advancing by \(\mathrm{d}a/\mathrm{d}N=C(\Delta K)^m\); dividing the Paris integral life \(N_f\) by a safety factor sets NDT inspection intervals that prevent sudden fatigue overload.

Next up — the Grand Finale of the Textbook: Creep, Residual Stress, Environmental Cracking & 13-Chapter Synthesis — Kê grain-boundary peak, Ashby deformation maps, landing-gear shot peening, hydrogen delayed fracture, and our 13-chapter symphony.

Fracture & Failure of Materials II
IN-CLASS QUIZ

Three Quick Questions: Click an Option to Check, or Launch a Live QR Poll

1. Which statement on fracture features and Cottrell cleavage nucleation is completely accurate?

River tributaries merge downstream while chevron V-tips point back to the origin; mating shear dimples point opposite whereas tear dimples point the same way.

2. Among solid-solution, precipitation, cold-work, and fine-grain strengthening, why does grain refinement alone lower DBTT in bcc steels?

Grain boundaries shorten pile-ups and deflect cleavage planes so \(k_f\gt k_y\), widening \(\sigma_f-\sigma_{\mathrm{ys}}\) and shifting DBTT downward.

3. ① For \(\sigma_e=250,\;\sigma_{\mathrm{UTS}}=600,\;\sigma_m=200\text{ MPa}\), find Goodman allowable \(\sigma_a\); ② for Paris \(m=4\), doubling \(\Delta\sigma\) changes life \(N_f\) to:

\(\sigma_a=250(1-200/600)\approx 166.7\text{ MPa}\); since \(N_f\propto(\Delta\sigma)^{-m}\), doubling \(\Delta\sigma\) at \(m=4\) cuts \(N_f\) to \(2^{-4}=1/16\).

Fracture & Failure of Materials II
FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 13 (PART 2)

Thank You

3 Embedded Models: DBTT Yield–Cleavage Competition (M12·02) · Fatigue S–N Curve & PSBs (M12·08) · Paris Fatigue Crack Growth Life (M12·04) — mse3d.com