FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 10

Solidification & Crystallization I

Homogeneous & Heterogeneous Nucleation, Jackson Factor, Supercooling & Crystal Growth
TEXTBOOK § 10.1 – § 10.3 · SOLIDIFICATION & CRYSTALLIZATION · PART 1
“Pile up earth into a mountain, and wind and rain will rise from it; gather water into a chasm, and dragons will be born within. Without accumulating half-steps, one cannot reach a thousand miles; without gathering tiny streams, no river or sea can form.”Xunzi · Classical Philosopher of the Late Warring States Period
Liang Wumse3d.com · Smart Classroom
Top: spherical-cap heterogeneous nucleation overcoming ΔG*·f(θ) · Bottom: continuous rotational symmetry breaking into a 6/mmm snowflake dendrite
ClickWheel→ NextP PenL LaserO OverviewF FullB Blank
PROLOGUE · PHASE DIAGRAMS FIX ENDPOINTS; CH. 10 OPENS OUR FIRST “DRIVING FORCE × PATHWAY × RATE” TRANSFORMATION

Why Does Pure Water Stay Liquid at \(-40\,^\circ\mathrm{C}\), and Why Never Cubic Snowflakes?

QUESTION 1 · LIQUID PURE WATER AT −40 °C & IRON DROPLETS UNDERCOOLED BY 300 K

Once temperature drops below the equilibrium melting point \(T_{\mathrm{m}}\), solid already has lower bulk free energy than liquid—why can ultrapure water be cooled to \(-40\,^\circ\mathrm{C}\) and clean liquid-iron microdroplets undercool by \(\sim 300\text{ K}\) without freezing?

QUESTION 2 · A PINCH OF TiB₂ REFINES AN INGOT—WHY DOES HOLDING CAUSE “FADING”?

Adding just \(0.01\%\) \(\mathrm{TiB_2}\) inoculant turns coarse columnar aluminum ingots into fine equiaxed grains—why do fewer than \(1\%\) of particles actually nucleate grains, and why does prolonged holding before pouring cause “inoculation fade”?

QUESTION 3 · SIXFOLD SNOWFLAKES, CUBIC ROCK SALT & FACETED SILICON SINGLE CRYSTALS

Crystallizing alike from disordered fluids, why does ice always grow into sixfold dendritic snowflakes while \(\mathrm{NaCl}\) forms sharp cubes—and why are metallic solid–liquid interfaces atomically rough and rounded whereas semiconductor silicon grows flat facets?

Ch. 10 Prologue · Bridging Ch. 7 Diffusion & Ch. 9 Interfacial Energy
CHAPTER 10 (PART 1) · FIVE-STOP ROADMAP

Surmount the Interfacial Barrier First, Then Watch Attachment, Solute Pile-Up & Symmetry Carve Morphology

  1. Homog. Nucleation\(r^3\) bulk gain vs. \(r^2\) cost
    Bell-shaped rate \(I(\Delta T)\)
    § 10.1
  2. Heterog. NucleationSpherical cap & \(f(\theta)\) factor
    Refinement limit & recalescence
    § 10.2
  3. Growth & \(\alpha\) FactorCont. / 2D nucl. / screw spiral
    Jackson criterion \(\alpha = 2\)
    § 10.3.1–3
  4. Constit. SupercoolingBPS partition factor \(k_{\mathrm{eff}}\)
    \(G_L/v\) breakdown & \(G\text{–}v\) map
    § 10.3.2 & 4
  5. Dendrite · Eutectic · Epitaxy\(\langle 100\rangle\) tips & \(6/mmm\) snow
    \(\lambda^2 v = K_{\mathrm{JH}}\) & FM/VW/SK
    § 10.3.5–7
Ch. 10 Part 1 (§ 10.1–§ 10.3) · Template for Ch. 11 Solid-State Kinetics
01
PART I

Homogeneous & Heterogeneous Nucleation

Undercooled melts carry short-range order, yet nascent clusters are surface-dominated—only deep undercooling \(\Delta T\) or a wetted substrate lowers the \(\gamma^3/\Delta T^2\) barrier so embryos cross \(r^*\).
  1. Homogeneous free energy, critical radius \(r^*\), \(1/3\) surface rule & \(-40\,^\circ\mathrm{C}\) ice nucleus05
  2. Volmer bell-shaped steady-state nucleation rate \(I(T)\) & spherical-cap wetting factor \(f(\theta)\)06
  3. 3D model: nucleation barrier & critical nucleus + grain-refinement limit, recalescence & fade07
§ 10.1.1 – § 10.1.3 · SHORT-RANGE LIQUID ORDER, HOMOGENEOUS BARRIER & THE −40 °C ICE BENCHMARK

The Barrier Equals \(1/3\) of Critical Surface Energy and Plummets as \(\Delta G^* \propto \gamma^3/\Delta T^2\)

\(\begin{gathered}\Delta G(r)=\tfrac{4}{3}\pi r^3\Delta G_v+4\pi r^2\gamma,\quad \Delta G_v\approx -\frac{\Delta H_{\mathrm{m}}}{T_{\mathrm{m}}}\Delta T\\ r^*=-\frac{2\gamma}{\Delta G_v}=\frac{2\gamma T_{\mathrm{m}}}{\Delta H_{\mathrm{m}}\Delta T}\propto\frac{1}{\Delta T},\quad \Delta G^*=\frac{16\pi\gamma^3}{3\Delta G_v^2}=\tfrac{1}{3}(4\pi r^{*2}\gamma)\propto\frac{1}{\Delta T^2}\end{gathered}\)
  • Embryo vs. Nucleus & Shape Penalty: Clusters with \(r\lt r^*\) are subcritical embryos (remelting), whereas \(r\gt r^*\) are stable nuclei; at \(r^*\), bulk gain cancels \(2/3\) of surface cost (a cubic nucleus also obeys \(\Delta G^*_{\mathrm{cube}}=\tfrac{1}{3}A^*\gamma\), yet its barrier is \(6/\pi\approx 1.91\times\) higher than a sphere).
  • Answering Q1 (Ice Benchmark): In pure water at \(-40\,^\circ\mathrm{C}\) (\(\Delta T=40\text{ K}\)), \(r^*\approx 1.3\text{ nm}\) holds \(\approx 290\) \(\mathrm{H_2O}\) molecules (\(57\%\) in the outer shell) with \(\Delta G^*\approx 70\,k_{\mathrm{B}}T\). At \(\Delta T=5\text{ K}\), \(r^*\) grows \(8\times\), \(N^*\) swells \(512\times\) (\(\sim 1.5\times 10^5\) molecules), and \(\Delta G^*\) explodes \(64\times\)—impossible.
Fig. 10.1 & Ice Case: r³ Bulk vs. r² Surface Trade-Off (Left) & ΔT Scaling (Right) +4πr²γ (surface) (4/3)πr³ΔGv Barrier ΔG* = (1/3)A*γ r* Embryo shrinks Nucleus grows → Pure Water ΔT = 40 K (−40 °C) ~290 r* ≈ 1.3 nm ΔG* ≈ 70 kB T 57% in outer shell At ΔT = 5 K Only (−5 °C) r* × 8 (≈ 10.4 nm) N* × 512 (~150,000 H₂O) ΔG* × 64 (~4500 kB T) Clean metals: ΔTh ≈ 0.18 Tm
Textbook § 10.1.1–10.1.3 · Homogeneous Barrier & Ice Case (Eqs. 10.1–10.9, Fig. 10.1)
§ 10.1.4 & § 10.2.1 – § 10.2.2 · VOLMER STEADY-STATE RATE Iss(T) & SPHERICAL-CAP FACTOR f(θ)

Barrier Crossing vs. Viscosity Carves a Bell “Nose”; Wetting Cuts \(\Delta G^*\) by \(f(\theta)\) at Fixed \(r^*\)

\(\begin{gathered}I_{\mathrm{ss}}=Z\beta^* N_1\exp\!\left(-\frac{\Delta G^*}{k_{\mathrm{B}}T}\right)\propto\exp\!\left(-\frac{\Delta G^*}{k_{\mathrm{B}}T}\right)\exp\!\left(-\frac{Q}{k_{\mathrm{B}}T}\right)\\ r^*_{\mathrm{het}}=r^*_{\mathrm{hom}},\quad \Delta G^*_{\mathrm{het}}=\Delta G^*_{\mathrm{hom}}\cdot\frac{(2+\cos\theta)(1-\cos\theta)^2}{4}\end{gathered}\)
  • Bell Curve & Metallic Glass: Small \(\Delta T\) lacks driving force while deep undercooling freezes diffusion \(\mathrm{e}^{-Q/k_{\mathrm{B}}T}\), peaking at nose \(T^*\) (\(d\approx(v/I)^{1/4}\)); quenching past the nose within incubation time \(\tau\) vitrifies liquid into metallic glass.
  • Spherical-Cap Factoring Miracle: Plugging Young's equation into cap volume and net interfacial energy factors out the same \(f(\theta)\)—curvature radius \(r^*\) stays unchanged, while atom count and barrier both scale by \(f(\theta)\) (\(90^\circ\to 0.5\), \(45^\circ\to 5.8\%\), \(30^\circ\to 1.3\%\)).
Tune contact angle \(\theta\) (cap tab): Nose T*
Textbook § 10.1.4 & 10.2.1–10.2.2 · Volmer Rate & Cap f(θ) (Eqs. 10.10–10.18)
§ 10.2.3 · INOCULATION LIMIT dmin ∼ (fact Nd)^(−1/3), RECALESCENCE & 3D NUCLEATION MODEL

Latent-Heat Recalescence Limits Activation to \(0.01\%\text{–}1\%\); Settling Fade Demands Late-Stream Inoculation

\(\begin{gathered}N_{\max}\approx f_{\mathrm{act}}N_d,\quad d_{\min}\sim N_{\max}^{-1/3}\\ \mathrm{TiB_2}:\;10^{14}\text{ m}^{-3}\!\times 1\%\implies d_{\min}\sim 100\;\mu\text{m}\end{gathered}\)
  • Answering Q2 Part 1 (Why \(<1\%\) Efficiency?): By Gibbs–Thomson curvature, free growth past a particle edge needs \(\Delta T\propto 1/d_{\mathrm{p}}\), so the coarsest \(\mathrm{TiB_2}\) particles activate first; their latent heat reheats the melt (recalescence), choking off the remaining \(99\%\) finer particles.
  • Answering Q2 Part 2 (Inoculation Fade): Holding \(\mathrm{Al\text{–}5Ti\text{–}1B}\) or \(\mathrm{Zr}\)-treated \(\mathrm{Mg}\) lets inoculants agglomerate and settle, coarsening grains—solved industrially by in-launder / late-stream inoculation right before pouring.
Textbook § 10.2.3 · Inoculants, Recalescence & Fade (Eq. 10.19)
02
PART II

Atomic Growth Mechanisms & Solute Partitioning

Once past \(r^*\), how does the interface advance? Monolayer bond-vs.-entropy competition sets Jackson's roughness factor \(\alpha\), while rejected-solute boundary layers reshape the effective partition coefficient \(k_{\mathrm{eff}}\).
  1. Continuous, 2D-nucleation & screw-spiral growth laws + Jackson \(\alpha = 2\) roughening model09
  2. Solute redistribution, diffusion boundary layer & Burton–Prim–Slichter (BPS) \(k_{\mathrm{eff}}\)10
§ 10.3.1 & § 10.3.3 · CONTINUOUS / LATERAL STEP GROWTH & JACKSON FACTOR α = (ΔS_m/R)(Z_s/Z)

\(\alpha \lt 2\) Yields Rough Metallic Fronts (\(v\propto\Delta T\)); \(\alpha \gt 2\) Yields Smooth Facets (\(\mathrm{Si}\) & Graphite)

\(\begin{gathered}\frac{\Delta G_{\mathrm{s}}}{Nk_{\mathrm{B}}T_{\mathrm{m}}}=\alpha x(1-x)+x\ln x+(1-x)\ln(1-x)\\ \alpha=\frac{\Delta S_{\mathrm{m}}}{R}\frac{Z_{\mathrm{s}}}{Z}:\;\alpha\lt 2\;(v\propto\Delta T)\;\text{vs.}\;\alpha\gt 2\;\bigl(v\propto(\Delta T)^2\bigr)\end{gathered}\)
  • Answering Q3 Part 2 (Rounded Metals vs. Faceted \(\mathrm{Si}\)): Metals have \(\Delta S_{\mathrm{m}}\approx R\Rightarrow\alpha\lt 2\) with a single well at \(x=0.5\) for continuous attachment everywhere; \(\mathrm{Si}\{111\}\) has \(\Delta S_{\mathrm{m}}/R=3.58\) and \(Z_{\mathrm{s}}/Z=3/4\), giving \(\alpha\approx \mathbf{2.7\gt 2}\)—minima split toward \(x\to 0,1\) into smooth facets growing via 2D nuclei or Frank screw spirals.
  • Ductile Iron Secret: Graphite (\(\alpha\approx 4\)) normally forms faceted flakes; trace \(\mathrm{Mg/Ce}\) poisons prism steps, forcing radial \(c\)-axis growth into spheroidal nodules.
Textbook § 10.3.1 & 10.3.3 · Jackson α Factor & Growth Laws (Eqs. 10.20–10.26)
§ 10.3.2 · STEADY-STATE BOUNDARY LAYER, BPS EFFECTIVE PARTITION COEFFICIENT keff & SOLUTE TRAPPING

Rejected Solute Piles Up to \(C_0/k_0\); Growth Rate & Stirring Tune \(k_{\mathrm{eff}}\in [k_0, 1]\) via \(v\delta/D_L\)

\(\begin{gathered}k_0=\frac{C_s^*}{C_L^*},\quad C_L(x)=C_0\!\left[1+\frac{1-k_0}{k_0}\mathrm{e}^{-vx/D_L}\right]\\ k_{\mathrm{eff}}=\frac{k_0}{k_0+(1-k_0)\exp(-v\delta/D_L)}\end{gathered}\)
  • Steady-State Spike: For \(k_0\lt 1\) (e.g., \(0.2\) in \(\mathrm{Fe\text{–}C}\), \(0.13\) in \(\mathrm{Al\text{–}Si}\)), steady-state freezing at \(C_s^*=C_0\) enriches interfacial liquid to \(C_0/k_0\), decaying exponentially over characteristic length \(D_L/v\).
  • BPS Limits & Rapid Solute Trapping: ① Slow + strong stirring (\(v\delta/D_L\to 0\)): \(k_{\mathrm{eff}}\to k_0\) maximizes purification (zone refining); ② Fast + stagnant (\(v\delta/D_L\to\infty\)): \(k_{\mathrm{eff}}\to 1\); ③ Ultrafast laser / splat: atoms cannot escape the advancing front, driving interfacial \(k_v\to 1\) (solute trapping into supersaturated solid solutions).
Drag Péclet number \(Pe = v\delta/D_L\) (\(k_0 = 0.20\)): vδ/D_L = 1.20
Textbook § 10.3.2 · Boundary Layer δ & BPS Formula (Eq. 10.22, Fig. 10.4)
03
PART III

Supercooling, Dendrites, Eutectics & Epitaxy

Solute pile-up depresses local liquidus ahead of the front—once thermal gradient \(G_L\) falls below the liquidus tangent, planar fronts break into cells and dendrites while eutectics and epitaxy select nanoscale lengths.
  1. Constitutional supercooling criterion \(G_L/v \lt \Delta T_0/D_L\) & 3D interface-instability model12
  2. Log–log \(G_L\text{–}v\) morphology map: from single-crystal blades & CZ silicon to laser AM13
  3. Cubic \(\langle 100\rangle\) dendrite selection, \(6/mmm\) snowflake symmetry breaking & Landau 1st-order rule14
  4. Regular coupled eutectics & Jackson–Hunt minimum-undercooling law \(\lambda^2 v = K_{\mathrm{JH}}\)15
  5. Thin-film epitaxy modes (FM / VW / SK) & self-assembled \(\mathrm{InAs/GaAs}\) quantum dots16
§ 10.3.4 · CONSTITUTIONAL SUPERCOOLING DERIVATION & 3D INTERFACE-INSTABILITY MODEL

Hotter Than the Front Yet Below Its Own Liquidus: \(G_L/v \lt \Delta T_0/D_L\) Triggers Breakdown

\(\begin{gathered}\left.\frac{\mathrm{d}T_L}{\mathrm{d}x}\right|_0=-\frac{m_L v C_0(1-k_0)}{k_0 D_L}=\frac{\Delta T_0}{D_L/v}\\ \text{Supercooling criterion: }\frac{G_L}{v}\lt\frac{|m_L|C_0(1-k_0)}{k_0 D_L}=\frac{\Delta T_0}{D_L}\end{gathered}\)
  • How Stringent Is Planar Growth?: For \(\Delta T_0=10\text{ K}\) and \(D_L=10^{-9}\text{ m}^2/\text{s}\), planar stability demands \(G_L/v \ge \mathbf{10^{10}\text{ K·s/m}^2}\). Below this threshold, any slight bulge pokes into undercooled liquid ahead and shoots forward.
  • Four-Stage Sequence: Zero supercooling (planar) \(\to\) narrow zone (cellular) \(\to\) transitional cellular dendrites \(\to\) wide, deep undercooled zone (branched columnar / equiaxed dendrites).
Textbook § 10.3.4 · Constitutional Supercooling Criterion (Eqs. 10.27–10.29, Fig. 10.6)
§ 10.3.4 · THE GL–v SOLIDIFICATION MAP: G_L/v SETS MORPHOLOGY; GL·v SETS SCALE.

Slope \(+1\) Lines Divide Planar / Cellular / Dendritic; Hunt's \(G_L^3/v\) Line Cuts Out Equiaxed

\(\begin{gathered}\frac{G_L}{v}\;\text{(morphology ratio: high}\to\text{planar, low}\to\text{dendritic / equiaxed)}\\ R_{\mathrm{c}}=G_L\cdot v\;\text{(cooling rate: higher toward upper-right}\to\text{finer scale)}\end{gathered}\)
  • Why Are Single-Crystal Blades Dendritic While CZ Silicon Is Planar? Directional superalloys (\(G_L/v\sim 10^7\)) still sit \(2\text{–}3\) orders below the alloy planar threshold (\(10^{10}\)), growing as aligned columnar dendrites; Czochralski high-purity \(\mathrm{Si}\) has \(C_0\to 0\), collapsing the threshold to zero for flat planar growth.
  • Casting vs. Additive Manufacturing: Sand casting sits in the low-\(G_L\) equiaxed zone; die casting chills & fragments dendrites to boost nuclei \(N\) into fine equiaxed grains; laser powder-bed fusion (SLM) occupies the upper-right ultrafine cellular-columnar corner.
Textbook § 10.3.4 · Log–Log GL–v Map & Process Windows (Fig. 10.7)
§ 10.3.5 · PREFERRED ⟨100⟩ DENDRITE ORIENTATION, CAST TEXTURE & SNOWFLAKE SYMMETRY BREAKING

Slow Close-Packed Faces Point Tips Along \(\langle 100\rangle\); Snowflakes & \(\mathrm{NaCl}\) Break \(\mathrm{SO(3)}\) Symmetry

\(\begin{gathered}\text{Cubic growth anisotropy: }v_{\langle 100\rangle}\gt v_{\langle 110\rangle}\gt v_{\langle 111\rangle}\\ \text{Fluid }\mathrm{SO(3)}\text{ breaking}\longrightarrow\begin{cases}\text{Ice Ih }(6/mmm)\implies\text{sixfold snowflake dendrite}\\ \mathrm{NaCl}\;(m\bar{3}m,\;\alpha\gt 2)\implies\text{cubic faceted salt crystal}\end{cases}\end{gathered}\)
  • Why Do Both fcc & bcc Dendrites Branch Along \(\langle 100\rangle\)? In fcc, slowest close-packed \(\{111\}\) planes bound an octahedron whose six sharp vertices point along \(\langle 100\rangle\)! Primary trunks and orthogonal side arms race along \(\langle 100\rangle\), crowding out tilted grains so turbine blades align low-modulus \(\langle 100\rangle\parallel\) centrifugal axis.
  • Answering Q3 Part 1 (Snowflakes & Landau's 1st-Order Rule): Vapor freezing into ice \(\mathrm{Ih}\) reduces continuous rotational symmetry to hexagonal \(6/mmm\), amplifying \(0.3\text{ nm}\) lattice symmetry into millimeter snowflakes; because density-wave order parameters allow a Landau cubic term, freezing is strictly first-order—requiring undercooling and nucleation.
Fig. 10.8 & Symmetry Breaking: fcc {111} Octahedron → ⟨100⟩ (Left) & 6/mmm Ice (Right) (a) Cubic Metal ⟨100⟩ Cross Dendrite [100] [010] Slow {111} octahedron → ⟨100⟩ tips hcp Mg grows along basal ⟨112̄0⟩ (b) 6/mmm Ice vs. m3̄m NaCl NaCl Slow {100} cube Ice Ih 6-fold dendrite Fluid SO(3) → Crystal point group Landau cubic term ⇒ 1st-order nucleation
Textbook § 10.3.5 · ⟨100⟩ Selection & Symmetry Breaking (Fig. 10.8)
§ 10.3.6 · JACKSON–HUNT THEORY OF COUPLED EUTECTIC GROWTH (1966)

Lateral Diffusion \(\propto v\lambda\) vs. Curvature \(\propto 1/\lambda\) Locks In \(\lambda^2 v = K_{\mathrm{JH}}\) at Minimum \(\Delta T\)

\(\begin{gathered}\Delta T(\lambda)=\underbrace{K_1 v\lambda}_{\text{lateral diffusion}}+\underbrace{\frac{K_2}{\lambda}}_{\alpha/\beta\text{ curvature}}\\ \frac{\partial\Delta T}{\partial\lambda}=0\implies\lambda^2 v=\frac{K_2}{K_1}\equiv K_{\mathrm{JH}}\;\;(\lambda\propto v^{-1/2},\;\Delta T_{\min}\propto v^{1/2})\end{gathered}\)
  • Two Opposing Penalties: Coarse lamellae (large \(\lambda\)) stretch lateral solute-exchange paths between \(\alpha\) and \(\beta\); overly fine lamellae (small \(\lambda\)) pack dense \(\alpha/\beta\) interphase area, spiking Gibbs–Thomson curvature undercooling.
  • Engineering Scaling Law: In \(\mathrm{Pb\text{–}Sn}\) eutectic (\(K_{\mathrm{JH}}\approx 35\;\mu\text{m}^3/\text{s}\)), boosting growth velocity \(v\) by \(100\times\) refines lamellar spacing \(\lambda\) to \(1/10\), elevating strength and toughness together.
Drag solidification velocity \(v\) (\(K_{\mathrm{JH}} = 100\;\mu\text{m}^3/\text{s}\)): v = 4 μm/s
Textbook § 10.3.6 · Coupled Eutectics & Jackson–Hunt Law (Eqs. 10.30–10.31)
§ 10.3.7 · THIN-FILM EPITAXY: YOUNG WETTING & MISFIT STRAIN CO-SELECT FM / VW / SK MODES

Low-Misfit Wetting Grows Superlattices (FM); \(7\%\) Strain Self-Assembles Quantum Dots (SK)

\(\begin{gathered}\delta=\frac{2(a_f-a_s)}{a_f+a_s},\quad\gamma_s\gtrless\gamma_f+\gamma_{fs}\\ \mathrm{FM}\text{ layer}\;\mid\;\mathrm{VW}\text{ island}\;\mid\;\mathrm{SK}\text{ wetting layer + QDs}\end{gathered}\)
  • FM Layer-by-Layer vs. VW Island: When \(\gamma_s\gt\gamma_f+\gamma_{fs}\) with tiny misfit (e.g., \(\mathrm{Si/Si}\), \(\mathrm{AlGaAs/GaAs}\)), films wet completely monolayer by monolayer in MBE (FM); when \(\gamma_s\lt\gamma_f+\gamma_{fs}\) (e.g., \(\mathrm{Au/SiO_2}\)), adatoms bead directly into 3D islands (VW).
  • SK Layer-Plus-Island & Quantum-Dot Lasers: \(\mathrm{InAs/GaAs}\) (\(\delta=7\%\)) wets for \(\sim 1.7\) monolayers first, then relieves rising coherent bulk strain via free island sidewalls to self-assemble \(10\text{–}50\text{ nm}\) 3D-confined quantum dots.
Textbook § 10.3.7 · FM / VW / SK Epitaxy & Quantum Dots (Fig. 10.9)
SUMMARY

Barriers Govern Nucleation, \(\alpha\) Sets Roughness, and \(G_L/v\) Sculpts Planar-to-Dendritic Microstructures

Homog. Barrier γ³/ΔT²→Cap f(θ) & Recalescence→Jackson Criterion α = 2→Supercooling G_L/v→Eutectic λ²v & Epitaxy
ANSWERING QUESTIONS 1 & 2

Without foreign interfaces, pure water relies on homogeneous nucleation (\(-40\,^\circ\mathrm{C}\) still needs \(\approx 290\) molecules crossing \(70\,k_{\mathrm{B}}T\)). Small-\(\theta\) \(\mathrm{TiB_2}\) slashes the barrier by \(f(\theta)\), yet the coarsest particles activate first and release latent heat (recalescence) that suppresses the remaining \(99\%\); settling fade is solved by late-stream inoculation.

ANSWERING QUESTION 3

Disordered vapor breaks rotational symmetry into hexagonal \(6/mmm\) dendritic snowflakes, while \(\mathrm{NaCl}\) breaks into cubic \(m\bar{3}m\) with \(\alpha\gt 2\) cube facets; metals (\(\alpha\lt 2\)) grow continuously on atomically rough fronts, whereas \(\mathrm{Si}\{111\}\) (\(\alpha\approx 2.7\gt 2\)) grows smooth facets.

Next Lecture (From Mechanisms to Real Castings & 3D Printing) — Solidification & Crystallization II: three ingot zones & Hunt's CET, single-crystal grain selection, Scheil microsegregation, Chvorinov riser design, and laser additive manufacturing.

Solidification & Crystallization I
CONCEPT QUIZ

Three Quick Questions: Click an Option to Check or Launch a Live Class Poll

1. A metal has \(\gamma=0.1\text{ J/m}^2\), \(\Delta H_{\mathrm{m}}=10^9\text{ J/m}^3\), and \(T_{\mathrm{m}}=1500\text{ K}\). At \(\Delta T=300\text{ K}\), what is homogeneous \(r^*\)? At \(\theta=45^\circ\), how do heterogeneous \(r^*\) and \(f(\theta)\) behave?

\(|\Delta G_v|=10^9\times 300/1500=2\times 10^8\text{ J/m}^3\) gives \(r^*=2\gamma/|\Delta G_v|=1.0\text{ nm}\); wetting leaves \(r^*\) unchanged while \(f(45^\circ)\approx 5.8\%\).

2. An alloy (\(C_0=2\%\), \(k_0=0.3\), \(m_L=-5\text{ K/}\%\), \(D_L=10^{-9}\text{ m}^2/\text{s}\)) solidifies at \(v=10^{-4}\text{ m/s}\). What minimum \(G_L\) avoids supercooling, and how does eutectic \(\lambda\) scale if \(v\) rises \(100\times\)?

\(\Delta T_0=|m_L|C_0(1-k_0)/k_0=23.3\text{ K}\), so \(G_L\ge v\Delta T_0/D_L=2.33\times 10^6\text{ K/m}\); from \(\lambda^2 v=K_{\mathrm{JH}}\), \(100\times\) faster \(v\) refines \(\lambda\) to \(1/10\).

3. Which statement regarding Jackson's roughness factor \(\alpha\) and thin-film heteroepitaxial growth modes is completely accurate?

Metals have \(\alpha\lt 2\) (rough continuous growth), whereas \(\mathrm{Si}\{111\}\) has \(\alpha\approx 2.7\gt 2\) (faceted); \(7\%\) misfit strain triggers SK quantum-dot assembly.

Solidification & Crystallization I
FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 10 (PART 1)

Thank You

4 Embedded Models: Nucleation Barrier & Critical Nucleus · Jackson α Factor · Constitutional Supercooling · Epitaxial Growth Modes — mse3d.com