FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 10 FINALE

Solidification & Crystallization II

Ingot Zones, Single-Crystal Selection, Scheil Segregation, Casting Defects & Additive Manufacturing
TEXTBOOK § 10.4 – § 10.6 · INGOT ZONES, SINGLE CRYSTALS, SCHEIL SEGREGATION & AM · PART 2
“Only by uniting microscale solute partitioning, dendritic growth, and mushy-zone fluid flow up to the engineering scale did foundry casting evolve from an ancient craft into a predictive quantitative science.”Fundamentals of Materials Science · Ch. 10 · In Tribute to M. C. Flemings & Zhou Yaohe
Liang Wumse3d.com · Smart Classroom
Top: spiral grain selector filters out a single-crystal turbine blade · Bottom: SLM laser melt pool & cross-layer epitaxial columnar grains
ClickWheel→ NextP PenL LaserO OverviewF FullB Blank
OPENING · FROM NUCLEATION & COMPETITIVE GROWTH TO INGOTS, FURNACES & LASER POOLS

How Does a Spiral Tube Select One Crystal, and Why Does \(10^6\text{ K/s}\) 3D Printing Grow Coarse Columns?

QUESTION 01 · EQUIAXED INGOTS VS. BOUNDARY-FREE TURBINE BLADES

Metal-mold ingots freeze inward into chill, columnar, and central equiaxed zones; structural ingots expand the equiaxed zone to prevent hot cracking, yet how does a single helical tube filter an entire jet-engine turbine blade into one crystal?

QUESTION 02 · WHY DOES SUB-SOLUBILITY Al–4.5%Cu ALWAYS FORM EUTECTIC?

\(\mathrm{Al\text{–}4.5\%Cu}\) sits well below the \(5.65\%\) equilibrium solubility limit and should freeze into single-phase \(\alpha\)—why do real castings always retain low-melting interdendritic eutectic films that trigger intergranular hot tearing?

QUESTION 03 · WHY DOES MILLION-KELVIN-PER-SECOND SLM GROW CROSS-LAYER COLUMNS?

Selective laser melting (SLM) cools at \(10^5\text{–}10^6\text{ K/s}\)—six to seven orders faster than sand casting—so why do uninoculated builds grow coarse \(\langle 001\rangle\) columnar grains spanning dozens of layers instead of fine equiaxed grains?

Textbook § 10.4 – § 10.6 · Ingots, SX Blades, Scheil Segregation & Metal AM
CHAPTER 10 (PART 2) · FIVE-STOP LECTURE ROADMAP

From Ingot Three-Zone Control & Single-Crystal Growth to Scheil Segregation, Casting Defects & 3D Printing

  1. Three Zones & CETChill · columnar · equiaxed
    Hunt criterion \(G^n/v\)
    § 10.4.1
  2. SX & Rapid CastingBridgman & spiral selector
    Pfann FZ · CC · melt-spin
    § 10.4.2–4
  3. Scheil & SDAS\(C_s^* = k_0 C_0(1-f_s)^{k_0-1}\)
    Cooling ruler \(\lambda_2\propto R_{\mathrm{c}}^{-1/3}\)
    § 10.5.1
  4. Macroseg. & DefectsFlemings A / V segregates
    Chvorinov risers & hot tears
    § 10.5.2–4
  5. Welding & Metal AMWeld FZ & 3 HAZ subzones
    SLM epitaxy & CET control
    § 10.6
Chapter 10 · Part 2 (§ 10.4 – § 10.6) · Solidification Physics in Engineering
01
PART ONE

Ingot Three-Zone Control, Single Crystals & Rapid Casting

The same competitive growth and Hunt \(G^n/v\) criterion work both ways: lower \(G^n/v\) to refine heavy ingots into dense equiaxed grains, or raise it to grow boundary-free turbine blades and \(300\text{ mm}\) silicon boules.
  1. Ingot three-zone structure & Hunt's quantitative CET criterion05
  2. Bridgman directional solidification, spiral selector model & three generations of turbine blades06
  3. Pfann zone refining, continuous-casting \(\sqrt{t}\) shell law & melt-spun rapid solidification07
§ 10.4.1 & EXTENDED READING · INGOT THREE-ZONE STRUCTURE & HUNT'S CET CRITERION

Equiaxed Fraction Above \(49\%\) Blocks Columns: Raising \(N\) \(1000\times\) Lifts \(G_{\mathrm{crit}}\) \(10\times\)

\(\begin{gathered}G\gt G_{\mathrm{crit}}=\frac{1}{n+1}\!\left[\frac{4\pi N}{3\ln[1/(1-\phi)]}\right]^{1/3}\!\left(\frac{v}{a}\right)^{1/n}\iff\frac{G^n}{v}\gt\mathrm{const}\\ (\phi\approx 0.49\text{ fully equiaxed},\;\;\phi\approx 0.0066\text{ fully columnar},\;\;G_{\mathrm{crit}}\propto N^{1/3})\end{gathered}\)
  • Origin of the Three Ingot Zones: ① Outer chill zone (intense mold chilling drives high-\(\Delta T\) heterogeneous nucleation of fine equiaxed grains); ② Columnar zone (\(\langle 100\rangle\) competitive growth against heat flow; full transcrystallization creates a weak center impingement plane prone to hot-forging cracks); ③ Central equiaxed zone (falling \(G\), wide constitutional supercooling + detached dendrite arms boost \(N\) to block columns).
  • Three Levers to Expand Equiaxed Grains: Low-superheat pouring (prevents nucleus remelting) + in-stream inoculation (\(N\times 1000\) lifts \(G_{\mathrm{crit}}\) \(10\times\)) + electromagnetic stirring (EMS) to fragment dendrite arms.
Textbook § 10.4.1 · Ingot Three Zones & Hunt CET Criterion (Eq. 10.32, Fig. 10.10)
§ 10.4.2 · BRIDGMAN FURNACE, THREE SX PRINCIPLES & THREE GENERATIONS OF BLADES

High \(G/v\) Suppresses Stray Nuclei, Starter Competition Picks \(\langle 100\rangle\), and a Spiral Passes One Crystal

\(\begin{gathered}\text{Three SX rules: single seed/selector}\cdot\text{unidirectional heat}\cdot\text{high }G/v\\ \text{Equiaxed }(980\,^\circ\mathrm{C})\to\text{DS columnar }(1020\,^\circ\mathrm{C})\to\text{SX }(1150\,^\circ\mathrm{C}+)\end{gathered}\)
  • Answering Q1 (Two Industrial SX Routes): Semiconductors use Czochralski (CZ) seed pulling with Dash necking to expel dislocations in \(300\text{ mm}\) \(\mathrm{Si}\) boules; superalloy blades place a starter block + spiral grain selector at the Bridgman chill base, combining \(\langle 100\rangle\) overgrowth with geometric wall blocking to pass a single crystal.
  • Three-Generation Blade Leap: Directional solidification (DS) first eliminates transverse grain boundaries perpendicular to centrifugal stress; single-crystal (SX) blades eliminate all grain boundaries to eradicate high-\(T\) GB sliding and creep cavitation.
Textbook § 10.4.2 · Bridgman DS, CZ Pulling & Spiral SX Blades (Fig. 10.11)
§ 10.4.2–10.4.4 · PFANN ZONE REFINING, CONTINUOUS CASTING & RAPID SOLIDIFICATION

Zone Refining Sweeps Solute to the Tail; CC Shells Grow as \(\sqrt{t}\), and \(10^6\text{ K/s}\) Traps Metallic Glass

\(\begin{gathered}\text{Pfann single pass: }C_s(x)=C_0\!\left[1-(1-k_0)\exp\!\left(-\frac{k_0 x}{l}\right)\right]\\ \text{Continuous-casting shell law: }\delta_{\mathrm{shell}}\propto\sqrt{t}\;\;(\gt 95\%\text{ of world steel})\end{gathered}\)
  • 11N Electronic-Grade Silicon Duo (Case): Impurities with \(k_0\ll 1\) (\(\mathrm{Fe,Cu}\)) sweep readily to the tail via multi-pass crucible-free float-zone (FZ) refining; however, boron in \(\mathrm{Si}\) has \(k_0\approx 0.8\approx 1\) and resists zone refining, requiring chemical Siemens CVD purification before FZ.
  • CC Soft Reduction & Rapid Solidification Triad: Continuous casting applies crater-end soft reduction + EMS to suppress centerline segregation; copper-wheel melt spinning (\(10^6\text{ K/s}\)) yields supersaturated solid solutions, nanocrystalline/amorphous cores, and metastable phases (\(\mathrm{Nd\text{–}Fe\text{–}B}\)).
Textbook § 10.4.2–10.4.4 · Pfann Zone Refining, CC & Rapid Freezing (Fig. 10.12)
02
PART TWO

Solidification Segregation & Casting Defect Control

Negligible solid diffusion freezes solute partitioning into micron-scale dendritic coring (Scheil equation), mushy-zone flow creates decimeter A/V macrosegregation, and solidification shrinkage plus terminal liquid films govern Chvorinov risers and Zhou Yaohe's hot-tearing theory.
  1. Microsegregation, Gulliver–Scheil equation, \(\mathrm{Cu\text{–}Ni}\) calculation & interactive model09
  2. Secondary dendrite arm spacing \(\lambda_2 \propto R_{\mathrm{c}}^{-1/3}\) ruler & Flemings A / V macrosegregation10
  3. Shrinkage cavities, Chvorinov riser design, \(\mathrm{H_2}\) pinholes & Zhou Yaohe's hot-tearing theory11
§ 10.5.1 · MICROSEGREGATION (CORING) & THE GULLIVER–SCHEIL EQUATION (1942)

Zero Solid Diffusion Freezes Layers in Place: \(f_s\to 1\) Hits \(C_E\) to Precipitate Non-Equilibrium Eutectic

\(\begin{gathered}(1-f_s)\,\mathrm{d}C_L=(1-k_0)C_L\,\mathrm{d}f_s\\ C_s^*=k_0 C_0(1-f_s)^{k_0-1},\;\;\bar{C}_s=\frac{C_0}{f_s}\bigl[1-(1-f_s)^{k_0}\bigr]\end{gathered}\)
  • Answering Q2 (Non-Equilibrium Eutectic & Incipient Melting): For \(k_0\lt 1\), late-stage \(C_L\) surges to \(C_E\), leaving low-melting eutectic films between \(\mathrm{Al\text{–}4.5\%Cu}\) dendrites; homogenization annealing (\(t\sim\lambda_2^2/D_s\)) must start strictly below \(T_E\) to avoid incipient melting (overburning).
  • \(\mathrm{Cu\text{–}30\%Ni}\) Reverse Coring (\(k_0=1.4\gt 1\)): Dendrite cores freeze enriched in high-\(T_{\mathrm{m}}\) \(\mathrm{Ni}\) (\(42\%\)); at \(f_s=0.5\), \(C_L=22.7\%\), \(C_s^*=31.8\%\), and \(\bar{C}_s=37.3\%\).
Textbook § 10.5.1 · Gulliver–Scheil Equation & Cu–Ni Coring (Eqs. 10.33–10.35)
§ 10.5.1 – § 10.5.2 · SDAS COOLING RULER & HEAVY-INGOT MACROSEGREGATION

Ostwald Coarsening Sets the \(\lambda_2\) Cooling Ruler; Macrosegregation Takes \(4\times 10^6\times\) Longer to Diffuse

\(\begin{gathered}t_{\mathrm{O}}\propto\frac{\lambda_2^3}{D_L d_0}\sim t_{\mathrm{f}}\propto\frac{1}{R_{\mathrm{c}}}\implies\lambda_2=K_{\mathrm{DAS}}\,R_{\mathrm{c}}^{-1/3}\\ \frac{t_{\mathrm{macro}}}{t_{\mathrm{micro}}}\sim\left(\frac{0.1\text{ m}}{50\;\mu\text{m}}\right)^2=2000^2=\mathbf{4\times 10^6\times!}\end{gathered}\)
  • Inferring Cooling Rate from One Micrograph: For \(\mathrm{Al}\) alloys, \(K_{\mathrm{DAS}}\approx 50\;\mu\text{m·(K/s)}^{1/3}\)—sand casting (\(0.1\text{ K/s}\)) gives \(\sim 100\;\mu\text{m}\), die casting (\(10^3\text{ K/s}\)) \(5\;\mu\text{m}\), and SLM (\(10^6\text{ K/s}\)) just \(\mathbf{0.5\;\mu\text{m}}\). Faster cooling refines \(\lambda_2\) and cuts homogenization time quadratically.
  • Flemings Macrosegregation Triad: Buoyant solute-rich liquid channels remelt dendrites into inclined A-segregates; settling equiaxed crystals shear and draw residual liquid into V-segregates; sinking solute-lean crystals pile into a bottom negative-segregation cone—uncurable by annealing, so flow must be suppressed during freezing.
Figs. 10.14 & 10.15: Ostwald SDAS Ruler λ₂ (Left) & Heavy-Ingot Macrosegregation (Right) (a) Al Alloy λ₂ = 50·Rc^(−1/3) Sand (0.1 K/s) ~100 μm Chill (10 K/s) ~25 μm Die (10³ K/s) ~5 μm SLM (10⁶ K/s) ~0.5 μm Fine arms dissolve → coarse grow Anneal time t ~ λ₂²/D_s drops fast (b) Heavy Steel Ingot Macrosegregation Pipe / +seg. A-bands V-seg. −Seg. cone Mushy-zone flow · uncurable by anneal
Textbook § 10.5.1–10.5.2 · SDAS Ruler & A/V Macrosegregation (Figs. 10.14–10.15)
§ 10.5.3 – § 10.5.4 · CHVORINOV'S RULE, PINHOLES & ZHOU YAOHE'S HOT-TEARING THEORY

A \(12\%\) Larger Riser Modulus \(M = V/A\) Freezes \(25\%\) Later; Late GB Liquid Films Trigger Hot Tearing

\(\begin{gathered}t_{\mathrm{f}}=C_{\mathrm{m}}\!\left(\frac{V}{A}\right)^2=C_{\mathrm{m}}M^2\;\;(\text{Case: }t_{\mathrm{r}}/t_{\mathrm{c}}=1.25\Rightarrow D=112\text{ mm})\\ \text{Bubble }r^*=\frac{2\gamma}{\Delta p}\;\mid\;\text{Hot tear: }f_s\in[90\%,99\%]\text{ GB film pulled apart}\end{gathered}\)
  • Feeding Shrinkage & Degassing Melts: The \(3\%\text{–}6\%\) solidification contraction is fed by high-modulus or insulating/exothermic risers (raising effective \(C_{\mathrm{m}}\)) to keep the pipe outside the casting; since solid \(\mathrm{Al}\) retains only \(5\%\text{–}6\%\) of liquid \(\mathrm{H}\) solubility, rotary degassing + oxide-film filtration eliminate \(\mathrm{H_2}\) pinholes.
  • Zhou Yaohe's Hot-Tearing Mechanics & Mold Collapsibility: Near \(f_s=90\%\text{–}99\%\), bridged dendrites remain separated by thin Scheil liquid films—wider freezing ranges worsen tearing; boosting mold collapsibility, refining grains, and limiting \(\mathrm{S,P}\) prevent hot tears (whereas low-\(T\) solid stress causes cold cracking).
Riser \(D = H\) (casting \(100\times 100\times 200\text{ mm}\)): D = 112 mm
Textbook § 10.5.3–10.5.4 · Chvorinov Risers, Pinholes & Hot Tearing (Eq. 10.37)
03
PART THREE

Welding, Additive Manufacturing & Ch. 10 Synthesis

A weld pool is a traveling millimeter mini-ingot and a laser 3D-printing pool is a microsecond micro-ingot—the very same epitaxial competition, \(G/v\) ratio, and Hunt CET criterion unlock microstructure control in modern manufacturing.
  1. Weld-joint three-zone microstructure (FZ · three HAZ subzones · BM) & hot vs. cold cracking13
  2. Selective laser melting (SLM) cross-layer \(\langle 001\rangle\) epitaxy & nano-inoculated CET refinement14
  3. Chapter 10 master synthesis & bridge into Chapter 11 Solid-State Phase Transformations15
§ 10.6.1 · WELD-JOINT ZONES: EPITAXIAL FUSION ZONE + THREE HAZ SUBZONES

\(v\to 0\) at the Fusion Line Drives Epitaxial Columns; \(T_{\mathrm{peak}}(x)\) Carves Coarse-, Fine- & Intercritical HAZ

\(\begin{gathered}\text{Fusion line: }v\to 0,\;\;G\sim 10^4\text{–}10^6\text{ K/m}\implies\frac{G}{v}\to\infty\;(\text{epitaxial start})\\ \text{Weld centerline: }v\to v_{\mathrm{weld}},\;\;G\text{ drops}\implies\text{strong CS may nucleate equiaxed}\end{gathered}\)
  • Peak Temperature \(T_{\mathrm{peak}}\) Maps Three Zones & Five Bands: ① Fusion zone (FZ, \(\gt T_{\mathrm{m}}\)): epitaxial columns curve toward the centerline; ② Heat-affected zone (HAZ, \(A_1\text{–}T_{\mathrm{m}}\)): \(\gt 1100\,^\circ\mathrm{C}\) coarse-grained HAZ (runaway austenite growth—the weakest link), \(A_3\text{–}1100\,^\circ\mathrm{C}\) fine-grained HAZ (normalized refinement), and \(A_1\text{–}A_3\) intercritical HAZ; ③ Base metal (\(\lt A_1\)).
  • Two Distinct Weld Cracks: Centerline \(\mathrm{S,P}\) terminal liquid films pulled apart cause solidification hot cracking; rapid cooling of coarse-grained HAZ into brittle martensite plus diffusible \(\mathrm{H}\) triggers delayed H-induced cold cracking.
Fig. 10.16: Peak Temperature Tpeak(x) (Left) Maps onto Five Weld-Joint Zones (Right) Peak Temp. Tpeak Tm 1100° A₃ A₁ Closer to weld center → Weld-Joint Microstructural Bands ① Fusion Zone FZ (> Tm · Remelted Pool) Epitaxial columns · watch S/P hot cracking ② Coarse-Grained HAZ (1100 °C–Tm · Weakest) ③ Fine-Grained HAZ (A₃–1100 °C · Normalized) ④ Intercritical HAZ (A₁–A₃ · Partial γ) ⑤ Base Metal BM (< A₁ · Unaltered) HAZ = spatial gradient of solid-state transformations
Textbook § 10.6.1 · Weld FZ, Three HAZ Subzones & Cracking (Fig. 10.16)
§ 10.6.2 · METAL AM (SLM): CROSS-LAYER ⟨001⟩ EPITAXY & NANO-INOCULATED CET

Extreme \(G\sim 10^7\text{ K/m}\) Keeps \(G^n/v\) High for Cross-Layer \(\langle 001\rangle\) Columns; \(1\%\;\mathrm{TiB_2}\) Triggers CET

\(\begin{gathered}\text{SLM powder-bed pool: }R_{\mathrm{c}}\sim 10^5\text{–}10^6\text{ K/s},\;\;G\sim 10^6\text{–}10^7\text{ K/m}\\ \lambda_1\sim 0.5\;\mu\text{m}\text{ (dislocation cell walls)},\;\;G^n/v\gg\text{crit.}\implies\text{cross-layer }\langle 001\rangle\end{gathered}\)
  • Answering Q3 (Why Does Fast Cooling Grow Coarse Columns?): ① Each laser scan remelts the underlying layer top for barrier-free cross-layer epitaxy; ② Although \(v\) is high, \(G\sim 10^7\text{ K/m}\) enters Hunt's law as \(G^n\) (\(n\approx 3.4\)), keeping \(G^n/v\) far above critical to suppress equiaxed nuclei and lock strong \(\langle 001\rangle\) anisotropy (while \(0.5\;\mu\text{m}\) intragranular cell walls impart high yield strength alongside high residual tensile stress).
  • Two Routes to Isotropic Equiaxed AM: Dope powder with \(1\%\;\mathrm{TiB_2/AlN/La_2O_3}\) nanoparticles to boost \(N\) by orders of magnitude, or tailor scan strategies to lower \(G^n/v\).
Textbook § 10.6.2 · SLM Cross-Layer ⟨001⟩ Epitaxy & CET Control (Fig. 10.17)
CHAPTER 10 FINALE · FOUR PHASE-TRANSFORMATION PILLARS LEADING INTO CHAPTER 11

Stepping into Solid-State Transformations Adds Elastic Strain \(\Delta G_{\mathrm{strain}}\) & Diffusionless Shear

Core DimensionLiquid–Solid Solidification Laws (Ch. 10)Inheritance & New Physics in Solid-State Transformations (Ch. 11)
Drive & Barrier\(|\Delta G_v|=\Delta H_{\mathrm{m}}\Delta T/T_{\mathrm{m}}\), \(\Delta G^*\propto\gamma^3/\Delta T^2\)Bulk drive must pay elastic strain energy \((\Delta G_v+\Delta G_{\mathrm{strain}})\), dictating plate/lath shapes & K–S orientation relations
Heterogeneous SitesSpherical-cap \(\Delta G^*_{\mathrm{het}}=f(\theta)\Delta G^*\), \(\mathrm{TiB_2}\) inoculation & recalescenceGrain boundaries, dislocations & vacancy clusters nucleate first; coherent \(\to\) semicoherent \(\to\) incoherent aging sequence
Kinetics & CurvesBell-shaped \(I_{\mathrm{ss}}(T)\), rough vs. terraced growth & Jackson–Hunt eutecticSluggish solid diffusion shapes classic isothermal TTT / continuous-cooling CCT “C-curves” and pearlite lamellae
Non-Eq. FreezingScheil coring \(C_s^*(f_s)\), solute trapping & melt-spun metallic glassesQuenching past the C-curve nose triggers sonic-speed cooperative diffusionless martensitic shear, or \(\partial^2 G/\partial x^2\lt 0\) spinodal decomposition
Symmetry BreakingContinuous fluid rotational group breaking permits cubic term \(\Rightarrow\) strictly first-orderLandau order parameter \(\xi\) unifies second-order ordering, ferroelectric/ferromagnetic domains & first-order martensite variants
Chapter 10 One-Sentence Takeaway: Undercooling \(\Delta T\) and contact angle \(\theta\) decide whether nuclei form; Jackson factor \(\alpha\) and constitutional supercooling \(G_L/v\) decide planar, cellular, or dendritic morphology; and Hunt's \(G^n/v\) criterion plus Scheil's equation govern ingots, single-crystal blades, and 3D-printed microstructures & defects.
Textbook Ch. 10 Synthesis · Bridging Solidification to Ch. 11 Transformations
SUMMARY

Tune \(G^n/v\) to Steer Equiaxed vs. Single Crystals, and Apply Scheil & Chvorinov Laws to Tame Defects & AM Pools

Ingot Zones & Hunt CET→Spiral-Selected SX Blades→Scheil Coring & SDAS→Chvorinov Risers & Hot Tears→Weld HAZ & Metal AM
ANSWERING QUESTIONS 01 & 02

Structural ingots combine low superheat and \(\mathrm{TiB_2}\) inoculation to boost \(N\) and expand the equiaxed zone via CET, whereas SX blades maintain high \(G/v\) to suppress stray nuclei and use a spiral selector to pass one \(\langle 100\rangle\) crystal; zero solid diffusion forces \(\mathrm{Al\text{–}4.5\%Cu}\) along Scheil enrichment to \(C_E\), leaving interdendritic eutectic films.

ANSWERING QUESTION 03

SLM laser pools remelt the underlying layer for barrier-free cross-layer epitaxy while extreme \(G\sim 10^7\text{ K/m}\) keeps Hunt's \(G^n/v\) high, growing multi-layer \(\langle 001\rangle\) columnar grains strengthened by \(0.5\;\mu\text{m}\) cell walls; adding \(1\%\;\mathrm{TiB_2}\) nanoparticles triggers CET into isotropic fine equiaxed grains.

Chapter 10 complete. Up next — Chapter 11 · Solid-State Phase Transformations: classification tree & Landau order parameter, precipitation aging & spinodal decomposition, steel pearlite/bainite/martensite & TTT/CCT curves.

Solidification & Crystallization II · End of Chapter 10
CONCEPT QUIZ

Three Quick Questions: Click to Check or Launch a Live Class Poll

1. For an alloy with \(C_0=1\%\) and \(k_0=0.2\), what is the interfacial solid concentration \(C_s^*\) under the Scheil equation at \(f_s=0.5\) and \(f_s=0.9\), and why do sub-solubility castings often show interdendritic eutectic?

\(C_s^*=0.2(1-f_s)^{-0.8}\) gives \(0.348\%\) at \(f_s=0.5\) and \(1.26\%\) at \(f_s=0.9\); as \(f_s\to 1\), \(C_L\) inevitably reaches \(C_E\) to precipitate non-equilibrium eutectic.

2. By Chvorinov's rule \(t_{\mathrm{f}}=C_{\mathrm{m}}(V/A)^2\), to make a riser freeze \(44\%\) slower than the casting (\(1.44\times\)), what minimum modulus ratio \(M_{\mathrm{r}}/M_{\mathrm{c}}\) is required? And what is the homogenization-time ratio between macrosegregation (\(0.1\text{ m}\)) and dendritic coring (\(50\;\mu\text{m}\))?

Modulus ratio \(=\sqrt{1.44}=1.20\times\); since diffusion time scales as \(L^2/D_s\), \((0.1 / 5\times 10^{-5})^2 = 2000^2 = 4\times 10^6\times\), making macrosegregation impossible to anneal out.

3. Regarding Pfann zone refining, spiral single-crystal selectors, and selective laser melting (SLM), which statement is completely accurate?

Zone refining requires \(k_0\) far from \(1\); spiral selectors forbid stray nuclei and block competing columns geometrically; nano-inoculants raise \(N\) in SLM to trigger CET.

Solidification & Crystallization II
FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 10 COMPLETE

Thank You

4 Embedded Models: Ingot Zones & Casting · Preferred Orientation & Competitive Growth · Scheil Equation & Coring · Melt-Pool Solidification (Welding & AM) — mse3d.com