FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 9

Interfaces & Interfacial Energy I

Interface Thermodynamics, Grain-Boundary Geometry, Interphase Coherency & Wulff Construction
TEXTBOOK § 9.1 – § 9.5 · INTERFACES & INTERFACIAL ENERGY · PART 1
“God made the bulk; surfaces were invented by the devil.”Wolfgang Pauli · 1945 Nobel Laureate in Physics
Liang Wumse3d.com · Smart Classroom
Top: cusped broken-bond γ(θ) polar plot & Wulff inner-envelope facets · Bottom: fcc Σ3 coherent twin …ABC-A-CBA… chevron mirror
ClickWheel→ NextP PenL LaserO OverviewF FullB Blank
PROLOGUE · PHASE DIAGRAMS FIX PHASES & FRACTIONS; INTERFACES DICTATE GRAIN SIZE & MORPHOLOGY.

Why Do Two-to-Three-Atom-Thick Transition Layers Govern Bulk Strength & Lifetime?

Question 1 · Why Do 10–30 ppm of Boron Double Hardenability?Why does adding merely \(10\text{–}30\text{ ppm}\) of boron double the hardenability of steel, whereas phosphorus or tin segregating to the very same grain boundaries triggers catastrophic intergranular temper embrittlement?
Question 2 · Lotus Beading vs. Glass Film Spreading?Why does a drop of pure water spread into a transparent film on clean silicate glass, yet roll off a lotus leaf as a near-spherical bead with a contact angle around \(160^\circ\)?
Question 3 · No Grain Boundaries in Single-Crystal Blades—Do Interfaces Still Matter?Without altering alloy chemistry or grain size, how can tuning grain-boundary character stop intergranular corrosion in stainless steel—and what interfaces let grain-boundary-free single-crystal turbine blades survive centrifugal creep at \(1100\,^\circ\mathrm{C}\)?
Dual Identity in the Master Formula: Energy Cost vs. Kinetic Pathway① Energy penalty: creating unit area costs interfacial energy \(\gamma\) (\(\mathrm{J/m^2}\)), governing nucleation barriers \(\Delta G^*\propto \gamma^3\) and coarsening; ② Kinetic pathway: short-range boundary migration \(v = M\cdot\Delta G_v\) provides a second evolution channel independent of long-range diffusion.
Textbook Ch. 9 Prologue · Bridging Chs. 6–8 to Chs. 10–13 Kinetics
CHAPTER 9 (PART 1) · FIVE-STOP ROADMAP

From Broken-Bond Thermodynamics & Capillary Curvature to Grain Boundaries, Twins & Wulff Shapes

  1. Surface & SegregationBroken bonds & surface excess \(G^\sigma\)
    Gibbs adsorption: \(\mathrm{B}\) vs. \(\mathrm{P/Sn}\)
    § 9.1.1–3
  2. Curvature & WettingGibbs–Thomson solubility surge
    Young's eq., lotus & thermal grooves
    § 9.1.4–5
  3. Low-Angle GBsTilt edge walls & twist screw grids
    Read–Shockley radian formula
    § 9.2
  4. High-Angle & TwinsDisordered core & CSL \(\Sigma\) values
    \(\Sigma 3\) coherent twin energy cusp
    § 9.3
  5. Interphase & WulffCoherency \(r^2\text{ vs. }r^3\) trade-off
    \(\gamma(\boldsymbol{n})\) plot & Wulff inner envelope
    § 9.4–9.5
Ch. 9 Part 1 (§ 9.1–§ 9.5) · Static Structure, Segregation & Wulff Shape
01
PART I

Interface Thermodynamics: Segregation, Curvature & Wetting

Projecting chemical potentials onto Gibbs's zero-thickness dividing surface yields the Gibbs adsorption isotherm, curved-interface Gibbs–Thomson solubility, and Young's wetting balance.
  1. Surface broken bonds, four interface classes & Gibbs adsorption (\(\mathrm{B}\) hardenability vs. \(\mathrm{P/Sn}\) embrittlement)05
  2. Curved interfaces: Laplace pressure \(\Delta p = 2\gamma/r\) & Gibbs–Thomson solubility surge06
  3. Wetting & Young's equation, lotus superhydrophobicity & grain-boundary thermal grooves07
§ 9.1.1 – § 9.1.3 · BROKEN BONDS, GIBBS DIVIDING SURFACE & GIBBS ADSORPTION ISOTHERM

Solutes That Lower \(\gamma\) (\(\mathrm{d}\gamma/\mathrm{d}\ln a \lt 0\)) Spontaneously Enrich Boundaries (\(\Gamma \gt 0\))

\(\begin{gathered}\gamma\equiv\left(\frac{\partial G}{\partial A}\right)_{T,p,n_i},\quad G^\sigma=\gamma A+\sum_i\mu_i n_i^\sigma\\ \mathrm{d}\gamma=-\sum_i\Gamma_i\,\mathrm{d}\mu_i\implies \Gamma=-\frac{1}{RT}\frac{\mathrm{d}\gamma}{\mathrm{d}\ln a}\end{gathered}\)
  • Four Interface Classes & Energy Scale: \(2\text{–}3\) atom-thick 2D transition zones where translational symmetry breaks (solid–vapor surface, solid–liquid front, hetero-phase interphase boundary, homo-phase misoriented grain boundary); typical metal surface energies lie in \(1\text{–}2\text{ J/m}^2\).
  • Why Opposite Effects from Segregation? (Check Separation Work \(2\gamma_{\mathrm{s}}-\gamma_{\mathrm{gb}}\)) ① Temper embrittlement: \(\mathrm{P,Sb,Sn,As}\) slash newly fractured \(\gamma_{\mathrm{s}}\) even more than \(\gamma_{\mathrm{gb}}\), collapsing cohesion into intergranular fracture; ② Answering Q1 (Boron steel): \(10\text{–}30\text{ ppm B}\) lowers austenite \(\gamma_{\mathrm{gb}}\), suppresses boundary ferrite nucleation to double hardenability, and strengthens cohesion.
Textbook § 9.1.1–9.1.3 · Surface Energy & Gibbs Adsorption (Eqs. 9.1–9.4)
§ 9.1.4 · CURVED INTERFACES: LAPLACE PRESSURE Δp = 2γ/r & GIBBS–THOMSON RELATION

Capillary Pressure \(2\gamma/r\) Lifts Chemical Potential: Solubility Surges \(11\times\) at \(r = 1\text{ nm}\)

\(\begin{gathered}\Delta p=\frac{2\gamma}{r}\implies\Delta\mu=\Delta p\,\Omega=\frac{2\gamma\Omega}{r}\\ C_{\mathrm{eq}}(r)=C_{\mathrm{eq}}(\infty)\exp\!\left(\frac{2\gamma\Omega}{r k_{\mathrm{B}}T}\right)\approx C_{\mathrm{eq}}(\infty)\!\left(1+\frac{2\gamma\Omega}{r k_{\mathrm{B}}T}\right)\end{gathered}\)
  • Textbook Capillary Benchmark: With \(\gamma=0.5\text{ J/m}^2\), \(\Omega=2\times 10^{-29}\text{ m}^3\), \(T=600\text{ K}\), capillary length \(r_0=2\gamma\Omega/(k_{\mathrm{B}}T)\approx \mathbf{2.4\text{ nm}}\) — at \(r=10\text{ nm}\) solubility rises \(27\%\) (linear \(24\%\)); at \(r=1\text{ nm}\) the exact exponential leaps to \(11\times\) (linear \(3.4\times\) breaks down completely).
  • Three Pillars Across Upcoming Chapters: ① Subcritical embryos (\(r\lt r^*\)) redissolve; ② Big eats small in Ostwald ripening (\(\bar{r}^3\propto t\)); ③ Dendrite-tip curvature undercooling \(\Delta T_r = 2\gamma T_{\mathrm{m}}/(\Delta H_{\mathrm{m}}r)\).
Drag small-particle radius \(r_1\) (vs. \(r_2 = 25\text{ nm}\)): r₁ = 2.4 nm
Textbook § 9.1.4 · Laplace Pressure & Gibbs–Thomson Relation (Eqs. 9.5–9.6)
§ 9.1.5 · WETTING, YOUNG'S EQUATION, LOTUS SUPERHYDROPHOBICITY & THERMAL GROOVES

Tangential Tug-of-War Along the Triple Line Decodes Lotus Beads, Brazing & Grooves

\(\begin{gathered}\gamma_{SV}=\gamma_{SL}+\gamma_{LV}\cos\theta\implies\cos\theta=\frac{\gamma_{SV}-\gamma_{SL}}{\gamma_{LV}}\\ \text{Groove: }\gamma_{\mathrm{gb}}=2\gamma_{\mathrm{s}}\cos\frac{\psi}{2}\;\;(\text{metals }\gamma_{\mathrm{gb}}/\gamma_{\mathrm{s}}\approx 1/3)\end{gathered}\)
  • Three Wetting Regimes: When \(\gamma_{SV}-\gamma_{SL}\ge\gamma_{LV}\), Young's equation has no root and liquid spreads completely (\(\theta=0^\circ\), e.g., water on clean high-\(\gamma\) silicate glass); \(0^\circ\lt\theta\lt 90^\circ\) wets; \(\gamma_{SL}\gt\gamma_{SV}\Rightarrow\theta\gt 90^\circ\) is non-wetting.
  • Answering Q2 (Lotus Effect): Low-energy epicuticular wax atop micro-papillae traps air cushions (Cassie state) so droplets touch only a few percent of solid tips—expanding wets liquid–vapor area, driving \(\theta^*\approx 160^\circ\) roll-off.
Textbook § 9.1.5 · Young's Equation, Lotus Effect & Thermal Grooves (Eq. 9.7)
02
PART II

Grain-Boundary Geometry: Dislocation Walls to Twins

Split at \(15^\circ\) misorientation: low-angle boundaries assemble ordered 1D dislocation arrays, whereas high-angle plateaus are carved by Coincidence Site Lattices (CSL) into deep \(\Sigma 3\) twin cusps.
  1. Dislocation primer & low-angle symmetric tilt walls / orthogonal twist screw grids09
  2. 3D model: stress cancellation & Read–Shockley formula \(\gamma_0\theta(A-\ln\theta)\)10
  3. High-angle disordered cores & Coincidence Site Lattice (CSL / \(\Sigma\)) model11
  4. Coherent twin boundaries: \(\cdots ABC\underline{A}CBA\cdots\) mirror stacking & \(\Sigma 3\) cusp12
§ 9.2.1 – § 9.2.2 · DISLOCATION PRIMER & LOW-ANGLE TILT / TWIST BOUNDARIES (θ < 15°)

1D Line Defects Build 2D Boundaries: In-Plane Axis Forms Edge Walls; Normal Axis Forms Screw Grids

\(\begin{gathered}\theta\approx\frac{b}{D}\iff D\approx\frac{b}{\theta}\quad(\theta\text{ in rad},\;\theta\lt 15^\circ)\\ \text{Line elastic energy }E_l\approx\alpha G b^2\;\;(\alpha\approx 0.5\text{–}1)\end{gathered}\)
  • Edge vs. Screw Dislocations: An edge dislocation (\(\perp\)) terminates an extra half-plane with Burgers vector \(\boldsymbol{b}\perp\) line; a screw dislocation has \(\boldsymbol{b}\parallel\) line with magnitude \(b\) of about one interatomic spacing.
  • Tilt vs. Twist Geometry: ① Symmetric tilt GB: grains counter-rotate by \(\pm\theta/2\) about an in-plane axis, inserting like-signed edge dislocations every \(D=b/\theta\); ② Twist GB: rotating by \(\theta\) about the boundary normal weaves two orthogonal sets of screw dislocations.
Fig. 9.5: Low-Angle Dislocation Arrays — (a) Tilt Edge Wall vs. (b) Twist Screw Grid (a) Tilt GB: Like-Signed Edge Wall D ≈ b/θ In-plane axis · Higher θ ⇒ denser ⊥ (b) Twist GB: Orthogonal Screw Grid Good registry in cells · Strain on screw lines Normal axis · Two orthogonal screw sets
Textbook § 9.2.1–9.2.2 · Tilt Walls, Twist Grids & D ≈ b/θ (Fig. 9.5)
§ 9.2.3 · WILLIAM SHOCKLEY & THE READ–SHOCKLEY FORMULA (1950)

Long-Range Stress Cancels Beyond \(D\): \(\gamma_{\mathrm{gb}} = \gamma_0\,\theta\,(A - \ln\theta)\) Rises Sublinearly

\(\begin{gathered}\gamma_{\mathrm{gb}}=\frac{1}{D}E_l=\frac{\theta Gb}{4\pi(1-\nu)}\ln\frac{D}{r_0}=\gamma_0\,\theta\,(A-\ln\theta)\\ \gamma_0=\frac{Gb}{4\pi(1-\nu)},\;\;A=\ln\frac{b}{r_0}\;\;(\theta\text{ MUST be in rad})\end{gathered}\)
  • Why Cut Off Stress Integration at \(D\)? Beyond distance \(D\) from the wall, periodic edge-dislocation stress fields cancel out; raising \(\theta\) packs more lines (\(\propto\theta\)) while shrinking each core's screening radius \(D=b/\theta\) (\(-\ln\theta\)), yielding a concave-down rising curve.
  • Radian Rule & Validity Limit: Plugging \(\theta\) in degrees gives absurd negative energies. For \(A=0.3\), the formal peak \(\theta^*=\mathrm{e}^{A-1}\approx 28.5^\circ\) lies well past core overlap (\(\gt 15^\circ\)), so \(\gamma_{\mathrm{gb}}\) rises monotonically across all LAGBs.
Textbook § 9.2.3 · Read–Shockley Formula & Radian Rule (Eqs. 9.8–9.9)
§ 9.3.1 – § 9.3.2 · HIGH-ANGLE DISORDERED CORES (θ > 15°) & COINCIDENCE SITE LATTICE (CSL)

General HAGBs Plateau in Energy, While Periodic Low-\(\Sigma\) Coincidences Carve Sharp Cusps

\(\begin{gathered}\Sigma\equiv\frac{V_{\mathrm{CSL}}}{V_{\mathrm{unit}}}\;\;(\text{smaller }\Sigma\implies\text{higher coincidence})\\ \text{Square }\langle 001\rangle:\;\theta=36.87^\circ\;\bigl(\tan\tfrac{\theta}{2}=\tfrac{1}{3}\bigr)\implies\mathbf{\Sigma 5}\end{gathered}\)
  • Disordered Core vs. Special Boundaries: Above \(15^\circ\), overlapping cores form a \(2\text{–}3\) atom disordered layer (metal \(\gamma_{\mathrm{gb}}\approx 0.3\text{–}1\text{ J/m}^2\)); random HAGBs (\(\Sigma\gt 29\)) act as fast paths for segregation, corrosion, and cracking, whereas \(\Sigma 3,\Sigma 5,\Sigma 7,\Sigma 9\) fit orderly.
  • Low \(\Sigma\) Alone Does Not Guarantee Low \(\gamma_{\mathrm{gb}}\): Boundary-plane inclination also matters—for fixed \(\Sigma 3\), slicing on \(\{111\}\) gives an ultralow-energy coherent twin, whereas off-\(\{111\}\) incoherent twins carry far higher energy.
Textbook § 9.3.1–9.3.2 · HAGB Cores & CSL Σ5 Geometry (Figs. 9.7–9.8)
§ 9.3.3 · TWIN BOUNDARIES: Σ3 MIRROR INTERFACES & STACKING REVERSAL IN FCC METALS

\(\cdots ABC\,\underline{A}\,CBA\cdots\) Carries One Local hcp Layer: Zero Broken Bonds & \(<\tfrac{1}{10}\,\gamma_{\mathrm{HAGB}}\)

\(\begin{gathered}\text{fcc }\{111\}\text{ twin stacking: }\cdots A\,B\,C\,\underline{\mathbf{A}}\,C\,B\,A\cdots\\ 60^\circ/\langle 111\rangle\iff 70.5^\circ/\langle 110\rangle\implies\mathbf{\Sigma 3}\\ \gamma_{\mathrm{twin,coh}}\approx\tfrac{1}{2}\gamma_{\mathrm{SF}}\lt\tfrac{1}{10}\gamma_{\mathrm{HAGB}}\end{gathered}\)
  • Why Half the Stacking-Fault Energy? Both immediate neighbors of mirror plane \(A\) are \(C\) layers, creating just one local \(CAC\) (hcp-like) triplet versus two in an intrinsic stacking fault—dropping \(\gamma_{\mathrm{twin,coh}}\) to \(\sim 0.01\text{–}0.05\text{ J/m}^2\).
  • Herringbone Chevron Signature: Viewed along \(\langle 110\rangle\), inclined \(\{111\}\) planes kink symmetrically across the mirror plane at \(70.5^\circ\) on both sides—forming straight annealing twin bands in \(\mathrm{Cu,Ni}\) and austenitic stainless steels.
Figs. 9.6 & 9.9: Deep Σ3 Cusp at 70.5° (Left) & ABC–A–CBA Chevron Mirror (Right) (a) fcc ⟨110⟩ Tilt Energy γgb(θ) LAGB < 15° HAGB plateau Σ3 cusp 70.5° 15° Misorientation θ (twin < 1/10 plateau) (b) Coherent Twin (Shared Mirror Plane) … A B C [A] C B A … No broken bonds · Zero strain · Lowest HAGB γ
Textbook § 9.3.3 · Coherent Σ3 Twin Stacking & Half-SFE Relation (Figs. 9.6 & 9.9)
03
PART III

Interphase Coherency, 0D–3D Defects & Wulff Shape

Across two distinct phases, lattice misfit \(\delta\) and particle size govern coherency loss, while anisotropic \(\gamma(\boldsymbol{n})\) carves equilibrium crystal polyhedra via Wulff's inner envelope.
  1. Coherent, semicoherent & incoherent interphase boundaries: misfit \(\delta\) & \(r^2\text{ vs. }r^3\) trade-off14
  2. Ni-base single-crystal superalloy \(\gamma/\gamma'\) rafts & Table 9.1 0D–3D defect hierarchy15
  3. Anisotropic \(\gamma(\boldsymbol{n})\) polar plot & 3D Wulff construction: \(\gamma_i/h_i = \text{const}\)16
§ 9.4.1 · COHERENT, SEMICOHERENT & INCOHERENT INTERPHASE BOUNDARIES: MISFIT δ & SIZE TRADE-OFF

Tiny Precipitates Stay Coherent (\(\propto r^2\)); Growing Past \(r_{\mathrm{crit}}\) Inserts Misfit Dislocations (\(\propto r^3\))

\(\begin{gathered}\delta=\frac{a_\beta-a_\alpha}{a_\alpha},\quad\text{misfit dislocation spacing }D\approx\frac{b}{\delta}\\ E_{\mathrm{int}}=4\pi r^2\gamma\;(\propto r^2)\quad\text{vs.}\quad E_{\mathrm{el}}=\tfrac{4}{3}\pi r^3\Delta g_{\mathrm{el}}\;(\propto r^3)\end{gathered}\)
  • Three Classes by Misfit \(\delta\): ① Coherent (\(\delta\lt 0.05\)): continuous planes across interface, ultralow \(\gamma\) but high elastic strain; ② Semicoherent (\(0.05\text{–}0.25\)): periodic misfit dislocations relieve long-range strain; ③ Incoherent (\(\delta\gt 0.25\)): HAGB-like, zero coherency strain but highest \(\gamma\).
  • Aging Sequence Decoder: \(\mathrm{Al\text{–}Cu}\) aging \(\mathrm{GP}\) (coherent) \(\to\theta''/\theta'\) (semicoherent) \(\to\theta\) (incoherent) reflects particles growing past \(r_{\mathrm{crit}} = 3(\gamma_{\mathrm{semi}}-\gamma_{\mathrm{coh}})/\Delta g_{\mathrm{el}}\).
Textbook § 9.4.1 · Lattice Misfit δ & Coherency-Loss Radius (Eq. 9.10, Fig. 9.10)
§ 9.4 EXTENDED READING & § 9.4.2 · SINGLE-CRYSTAL TURBINE BLADE γ/γ′ INTERFACES & 0D–3D DEFECT HIERARCHY

“Zero Grain Boundaries” Still Relies on Interfaces: \(70\%\) Cuboidal \(\gamma/\gamma'\) Rafts Defeat Creep

Dim.Typical DefectsThermodynamic & Geometric EssenceKey Engineering Effects
0D PointVacancy, interstitial, soluteOnly class with equilibrium concentration (entropy-stabilized)Diffusion, doping, solid-solution strengthening
1D LineEdge, screw, mixed disloc.Burgers vector \(\boldsymbol{b}\), line energy \(\propto Gb^2\) (non-eq.)Plastic slip, work hardening
2D PlanarGB, twin, interphaseOrdered 1D arrays (tilt/twist/misfit) or CSLHall–Petch, segregation, intergranular attack
3D BulkPrecipitate, pore, inclusion3D micro-domains bounded by 2D interfacesPrecipitation hardening vs. crack initiation
Dimensionality Escalation Rule: Only 0D point defects exist in thermal equilibrium; 1D–3D defect densities are set by processing history, with higher-D defects often built from ordered lower-D arrays.
Answering Q3 · Ni-Base Single-Crystal SuperalloysEliminating all HAGBs stops high-\(T\) boundary sliding and cavitation, while packing a \(70\%\) volume fraction of ordered \(\mathrm{L1_2}\) cuboidal \(\gamma'(\mathrm{Ni_3Al})\) precipitates separated by tens-of-nanometer \(\gamma\) channels.
Room-\(T\) \(|\delta|\lt 0.1\%\) Coherency \(\to 1100\,^\circ\mathrm{C}\) Interfacial Dislocation ArmorTuning \(\mathrm{Al/Ti}\) gives near-zero room-\(T\) misfit (no short-circuit diffusion paths), forcing dislocations to bow inside narrow \(\gamma\) corridors; at \(1100\,^\circ\mathrm{C}\) service (\(|\delta|\approx 0.1\%\text{–}0.5\%\)), dense interfacial misfit dislocation networks relieve stress onto \(\gamma/\gamma'\) rafts and block \(\gamma'\) cutting.
Textbook § 9.4 & Table 9.1 · Single-Crystal γ/γ′ Rafts & 0D–3D Defect Hierarchy
§ 9.5 · INTERFACIAL-ENERGY ANISOTROPY & THE WULFF CONSTRUCTION

Close-Packed Planes Cut Fewest Bonds into \(\gamma(\boldsymbol{n})\) Cusps; Inner Envelope Equates \(\gamma_i / h_i\)

\(\begin{gathered}\boldsymbol{n}\cdot\boldsymbol{r}=\gamma(\boldsymbol{n})\;\;(\text{Wulff inner envelope})\\ V=\tfrac{1}{3}\sum_i A_i h_i,\;\;E=\sum_i\gamma_i A_i\\ \implies \gamma_1/h_1=\gamma_2/h_2=\cdots=\text{const}\end{gathered}\)
  • Why Does Constant \(\gamma_i/h_i\) Give Equilibrium? Adding an atom onto facet \(i\) raises chemical potential by \(2\gamma_i\Omega/h_i\)—when \(\gamma_i/h_i\) is uniform across all faces, chemical potential is equalized everywhere! (Isotropic \(\gamma\) gives a sphere \(2\gamma/r\); sharp cusps lie closest to the origin and emerge as flat facets.)
  • Equilibrium vs. Kinetic Shapes: Annealed microvoids display Wulff facets, whereas cast dendrites and pinned grains mostly show growth-controlled kinetic shapes.
Textbook § 9.5 · Polar γ-Plot & Wulff Construction (Eq. 9.11, Fig. 9.11)
SUMMARY

Thermodynamics Governs Segregation & Curvature; Dislocations & CSL Set GB Energy; Wulff Shapes Crystals

Gibbs Adsorption Γ→Gibbs–Thomson 2γΩ/r→Young Wetting & Grooves→Read–Shockley & CSL Σ3→Coherency & Wulff Shape
ANSWERING QUESTIONS 1 & 2

Because \(\mathrm{d}\gamma_{\mathrm{gb}}/\mathrm{d}\ln a\lt 0\), \(10\text{–}30\text{ ppm B}\) segregates to austenite grain boundaries, lowering \(\gamma_{\mathrm{gb}}\) to suppress ferrite nucleation and double hardenability (whereas \(\mathrm{P/Sn}\) slash \(2\gamma_{\mathrm{s}}-\gamma_{\mathrm{gb}}\) into temper embrittlement). Clean glass has high \(\gamma_{SV}\) for \(\theta=0^\circ\) film spreading, while lotus wax + micro-papillae air cushions push \(\theta^*\approx 160^\circ\).

ANSWERING QUESTION 3 (SINGLE-CRYSTAL BLADES)

Eliminating high-angle grain boundaries in Ni-base single-crystal blades removes high-\(T\) sliding, while a \(70\%\) volume fraction of low-misfit \(\gamma/\gamma'\) coherent interfaces and \(1100\,^\circ\mathrm{C}\) misfit dislocation networks armor the blade against creep—“banishing GBs” maximizes engineered interphase boundaries.

Next Lecture (Setting Interfaces in Motion) — Interfaces & Interfacial Energy II: thermally activated migration, Cahn solute drag & breakaway, Zener pinning, grain-boundary engineering, and powder sintering.

Interfaces & Interfacial Energy I
CONCEPT QUIZ

Three Quick Questions: Click an Option to Check or Launch a Live Class Poll

1. A solute lowers grain-boundary energy at \(\mathrm{d}\gamma/\mathrm{d}\ln a = -0.015\text{ J/m}^2\). At \(T=1000\text{ K}\) (\(R=8.314\text{ J/(mol·K)}\)), what is the interfacial excess \(\Gamma\) (\(\text{mol/m}^2\)) and segregation sign?

From \(\Gamma = -(1/RT)(\mathrm{d}\gamma/\mathrm{d}\ln a)\), we find \(0.015/8314\approx +1.8\times 10^{-6}\gt 0\): energy-lowering solutes spontaneously enrich grain boundaries.

2. For a symmetric tilt boundary with \(b=0.25\text{ nm}\) at \(\theta=5^\circ\), what is the edge-dislocation spacing \(D\), and what unit must \(\theta\) take in \(\gamma_0\theta(A-\ln\theta)\)?

\(5^\circ = 0.0873\text{ rad}\), giving \(D\approx b/\theta\) \(= 0.25/0.0873\approx 2.86\text{ nm}\); \(\theta\) must be in radians—plugging degrees gives unphysical negative \(\gamma_{\mathrm{gb}}\).

3. Which statement regarding \(\Sigma 3\) twins, precipitate coherency during coarsening, and Wulff equilibrium shapes is completely accurate?

Incoherent \(\Sigma 3\) boundaries carry far higher \(\gamma\) than \(\{111\}\) coherent twins; strain \(\propto r^3\) drives semicoherency; low-\(\gamma_i\) cusps lie closest (\(h_i\)) to dominate facets.

Interfaces & Interfacial Energy I
FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 9 (PART 1)

Thank You

5 Embedded Models: Three-Tension Balance · Dislocation Walls & Read–Shockley · Coincidence Site Lattice & Σ · Coherent/Semicoherent/Incoherent Interfaces · Wulff Construction — mse3d.com