FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 8 FINALE

Phase Equilibria & Phase Diagrams III

Fe–C Phase Diagram, Engineering Alloys, Ternary Systems, CALPHAD & Ellingham Diagram
TEXTBOOK § 8.9 – § 8.13 · FE–C, CU/AL/TI, TERNARY, CALPHAD & ELLINGHAM · PART 3
“By our Act II master formula ‘Evolution = Driving Force × Pathway × Rate,’ a phase diagram maps the first factor: the farther an actual state sits from phase-diagram equilibrium, the greater the driving force for evolution.”Fundamentals of Materials Science · Ch. 8 From Roozeboom's Fe–C Diagram & Jin's Diffusion Multiples to Hillert's CALPHAD
Liang Wumse3d.com · Smart Classroom
Gibbs composition triangle liquidus projection: primary crystals move away from apex → join monovariant eutectic valley → freeze at four-phase invariant E
ClickWheel→ NextP PenL LaserO OverviewF FullB Blank
OPENING · APPLYING PHASE-DIAGRAM PRINCIPLES TO STEELS, AEROSPACE ALLOYS & MULTICOMPONENT DESIGN

One Fe–C Chart Governs a Century of Steelmaking; One Negative-Slope Carbon Line Fuels Blast Furnaces

QUESTION 01 · WHY DOES < 8% CEMENTITE SHATTER TOOL-STEEL TOUGHNESS?

When hypereutectoid \(1.2\%\text{ C}\) tool steel (AISI W1) cools slowly, proeutectoid cementite makes up only \(7.3\%\) by mass—why does it leave the entire billet brittle and unmachinable unless a spheroidizing anneal is performed first?

QUESTION 02 · WHY IS WATER-QUENCHED Al–4.4%Cu SOFT, YET HARD AT 160 °C?

Water-quenched carbon steel turns glass-hard instantly—so why is aerospace \(\mathrm{Al\text{–}4.4\%Cu}\) soft right after quenching from \(530\,^\circ\mathrm{C}\), reaching peak strength only after holding at \(160\,^\circ\mathrm{C}\) (artificial aging)?

QUESTION 03 · IF CARBON IS LESS OXYGEN-AVID AT 25 °C, HOW DOES COKE SMELT IRON & SILICON?

At room temperature both \(\mathrm{Fe_2O_3}\) and \(\mathrm{SiO_2}\) are far more stable than \(\mathrm{CO}\)—why does raising furnace temperature let coke reduce iron and silica ores, yet still fail to smelt metallic titanium?

Textbook § 8.9–8.13 · Fe–C, Cu/Al/Ti, Ternary, CALPHAD & Ellingham
CHAPTER 8 PART 3 · FIVE-STOP LECTURE ROADMAP

From the Binary Crown Jewel (Fe–C) to Ternary Space, CALPHAD & Extractive Pyrometallurgy

  1. Fe–C & Carbon SteelsPeritectic, eutectic & eutectoid; pearlite vs. boundary \(\mathrm{Fe_3C}\)§ 8.9.1–2
  2. Metastability & Cast IronsMetastable common tangent; white, gray, ductile, CGI & malleable§ 8.9.3
  3. Cu / Al / Ti Alloys\(\alpha\)-brass solid solution, \(\mathrm{Al\text{–}Cu}\) aging & \(\mathrm{Ti\text{–}6Al\text{–}4V}\) / \(\gamma\text{-TiAl}\)§ 8.10
  4. Ternary & StainlessGibbs triangle, Alkemade theorem, isopleths & Schaeffler map§ 8.11
  5. CALPHAD & EllinghamRedlich–Kister \(G^\phi\) optimization & carbothermic smelting§ 8.12–13
Chapter 8 · Part 3 (§ 8.9 – § 8.13) · Five-Stop Roadmap
01
PART ONE

The Fe–C Diagram: Master Blueprint of Steels & Cast Irons

Combining peritectic, eutectic, and eutectoid isotherms into Roozeboom's metastable \(\mathrm{Fe\text{–}Fe_3C}\) diagram—five fundamental phases and three critical lines govern steels and cast irons alike.
  1. Five phases, three invariants (\(1495/1148/727\,^\circ\mathrm{C}\)) & peritectic casting cracks05
  2. Slow-cooled eutectoid, hypoeutectoid & hypereutectoid steels + pearlite model06
  3. White cast iron transformed ledeburite & proof of metastable > stable solubility07
  4. Metastable \(\mathrm{Fe\text{–}Fe_3C}\) vs. stable \(\mathrm{Fe}\text{–graphite}\): four engineering cast irons08
§ 8.9.1 – § 8.9.2 · METASTABLE Fe–Fe₃C PANORAMA, CRITICAL LINES & THREE INVARIANT REACTIONS

\(2.11\%\text{ C}\) Divides Steels from Cast Irons Across \(1495,\) \(1148,\) and \(727\,^\circ\mathrm{C}\) Invariants

\(\begin{gathered}1495\,^\circ\mathrm{C}\;(J):\;L_{0.53}+\delta_{0.09}\to\gamma_{0.17}\;(\text{peritectic})\\ 1148\,^\circ\mathrm{C}\;(C):\;L_{4.30}\to\gamma_{2.11}+\mathrm{Fe_3C}\;(\text{ledeburite})\\ 727\,^\circ\mathrm{C}\;(S):\;\gamma_{0.77}\to\alpha_{0.0218}+\mathrm{Fe_3C}\;(\text{pearlite})\end{gathered}\)
  • fcc vs. bcc Carbon Solubility Contrast: Larger octahedral interstices let fcc austenite \(\gamma\) dissolve up to \(\mathbf{2.11\%\text{ C}}\) at \(E\) (\(<2.11\%\) steels; \(>2.11\%\) cast irons), whereas bcc ferrite \(\alpha\) dissolves at most \(\mathbf{0.0218\%\text{ C}}\) at \(727\,^\circ\mathrm{C}\).
  • Peritectic Slab Cracks & \(A_1/A_3/A_{\mathrm{cm}}\): In \(0.09\text{–}0.17\%\text{ C}\) steels, the \(\delta\to\gamma\) \(0.4\%\) volume contraction triggers continuous-casting shell cracks; \(A_1(727\,^\circ\mathrm{C})\), \(A_3(GS)\), and \(A_{\mathrm{cm}}(ES)\) anchor heat-treatment schedules.
Textbook § 8.9.1–8.9.2 · Roozeboom Fe–Fe₃C & Three Invariants
§ 8.9.2 · SLOW-COOLING PATHWAYS IN CARBON STEELS: EUTECTOID, MEDIUM-CARBON & HYPEREUTECTOID

Pearlite Is \(\sim 89\%\) Soft Ferrite Reinforced by Fine \(\mathrm{Fe_3C}\) Lamellae; Break Boundary Nets

\(\begin{gathered}\text{Pearlite }(0.77\%):\;f^\alpha=\frac{6.69-0.77}{6.69-0.0218}\approx 88.8\%\\ \text{0.40\% C}:\;f^{\alpha_{\mathrm{pro}}}=\frac{0.77-0.40}{0.77-0.0218}\approx 49.5\%\\ \text{1.2\% C}:\;f^{\mathrm{Fe_3C}_{\mathrm{II}}}=\frac{1.2-0.77}{6.69-0.77}\approx 7.3\%\end{gathered}\)
  • Medium-Carbon \(0.40\%\text{ C}\) Steel (AISI 1040 / 1045): Slow cooling forms \(\sim 50\%\) blocky proeutectoid \(\alpha\) + \(\sim 50\%\) pearlite (\(\sigma_{\mathrm{y}}\approx 280\text{ MPa}\); quenching & tempering elevates \(\sigma_{\mathrm{y}}\) to \(620\text{ MPa}\)).
  • Answering Q1 (\(1.2\%\text{ C}\) Boundary Network): Just \(7.3\%\) proeutectoid \(\mathrm{Fe_3C}_{\mathrm{II}}\) wets prior-\(\gamma\) grain boundaries as a continuous brittle shell; a spheroidizing anneal breaks the network into globules before machining.
Textbook § 8.9.2 · Carbon Steels, Pearlite & Spheroidizing Anneal
§ 8.9.2 – § 8.9.3 · WHITE CAST IRON TRANSFORMED LEDEBURITE & METASTABLE SOLUBILITY PROOF

Higher \(G^{\beta'}(\mathrm{Fe_3C})\) Tilts the Common Tangent Solute-Rich: Metastable Solubility Exceeds Stable

\(\begin{gathered}4.30\%\text{ C }(1148\,^\circ\mathrm{C}):\;f^\gamma=\frac{6.69-4.30}{6.69-2.11}\approx 52.2\%\\ \xrightarrow{727\,^\circ\mathrm{C}}\text{Transf. ledeburite: }f^{\mathrm{P}}=\frac{6.69-4.30}{6.69-0.77}\approx 40.4\%\\ G^{\beta'}(\mathrm{Fe_3C})\gt G^\beta(\mathrm{C_{gr}})\implies x_{\mathrm{meta}}^\gamma(2.11\%)\gt x_{\mathrm{eq}}^\gamma(2.08\%)\end{gathered}\)
  • Three White Cast Irons: Eutectic (\(4.30\%\)), hypoeutectic (\(3.0\%\), primary \(\gamma\) dendrites rejecting \(\mathrm{Fe_3C}_{\mathrm{II}}\)), and hypereutectic (\(5.0\%\), coarse primary \(\mathrm{Fe_3C}_{\mathrm{I}}\) laths) all end with continuous cementite in transformed ledeburite—hard, brittle wear parts (grinding balls, plowshares).
  • Universal Tangent Geometry (Fig. 8.23): Lifting the precipitate curve from stable \(\beta\) to metastable \(\beta'\) shifts the matrix tangent point rightward (\(\Delta x\gt 0\))—explaining \(E(2.11\%)\gt E'(2.08\%)\) and setting the supersaturation threshold for Ch. 11 GP zones.
Textbook § 8.9.2–8.9.3 · White Cast Irons & Metastable Solubility
§ 8.9.3 · STABLE VS. METASTABLE DUAL DIAGRAM: GRAPHITIZATION & FOUR ENGINEERING CAST IRONS

Two Eutectics Differ by Just \(6\,^\circ\mathrm{C}\) (\(1154\) vs. \(1148\,^\circ\mathrm{C}\)): Spheroidizing Graphite Rivals Cast Steel

Cast IronGraphite & RouteProperties & Signature Uses
Gray IronFlake · Slow cool + \(\mathrm{Si}\) graphitizerSharp tip notches (\(\sigma_{\mathrm{b}}\approx 200\text{ MPa}\)); best damping (machine beds)
Ductile IronNodular · Melt inocul. with \(\mathrm{Mg/Ce}\)Eliminates notch tips, \(\sigma_{\mathrm{b}}=400\text{–}900\text{ MPa}\); rivals steel (crankshafts)
CGIVermicular · Controlled residual \(\mathrm{Mg/Ce}\)Balances strength, toughness & thermal conductivity (diesel blocks)
MalleableTemper carbon · Annealed white iron\(\mathrm{Fe_3C\to Fe + C_{gr}}\) floccules; thin-wall castability + ductility (fittings)
Kinetics Selects the Diagram: Fast cooling or carbide formers (\(\mathrm{Mn,Cr}\)) follow metastable \(\mathrm{Fe\text{–}Fe_3C}\) into white iron (\(1148/727\,^\circ\mathrm{C}\)); slow cooling + \(\mathrm{Si}\) follows stable \(\mathrm{Fe}\text{–graphite}\) (\(C'=4.26\%,\) \(1154\,^\circ\mathrm{C}\); eutectoid \(0.68\%,738\,^\circ\mathrm{C}\)).
Fig. 8.24(b)–(e): Same Matrix — Graphite Morphology Dictates Strength & Ductility (b) Gray · Flake Sharp tip notches ~200 MPa Best damping (c) Ductile · Nodular +Mg/Ce inocul. 400–900 MPa Rivals cast steel (d) CGI · Vermicular Blunt stubby worms Strength + heat Diesel blocks (e) Malleable Annealed white iron Temper carbon Thin pipe fittings
Textbook § 8.9.3 · Dual Fe–C Diagram & Four Cast Irons (Fig. 8.24)
02
PART TWO

Cu / Al / Ti Alloys & Ternary Phase Diagrams

Step beyond binary steels into brass solid solutions, age-hardened Al–Cu, and Ti–Al aerospace alloys—then conquer ternary space via Gibbs triangles and the Schaeffler weld map.
  1. \(\mathrm{Cu\text{–}Zn}\) brasses, three-step \(\mathrm{Al\text{–}Cu}\) age hardening & \(\mathrm{Ti\text{–}Al}\) alloys10
  2. Gibbs composition triangle, \(f^*=4-P\) & Jin Zhanpeng's diffusion multiples11
  3. Ternary liquidus projection, Alkemade saddle theorem & crystallization model12
  4. Why isopleths forbid the lever rule & \(\mathrm{Fe\text{–}Cr\text{–}Ni}\) Schaeffler weld map13
§ 8.10 · NON-FERROUS ALLOY TRIO: Cu–Zn SOLID SOLUTION, Al–Cu PRECIPITATION & Ti–Al INTERMETALLICS

A Steeply Retreating Solvus Unlocks Aerospace \(\mathrm{Al\text{–}Cu}\): Quench Soft, Age Hard

  • ① \(\mathrm{Cu\text{–}Zn}\) Brasses (Solid Solution + Peritectic Cascade): \(<36\%\text{ Zn}\) (70/30 cartridge brass, C26000) is single-phase fcc \(\alpha\) for deep drawing; \(36\text{–}46\%\text{ Zn}\) (60/40 brass, C28000) adds hard ordered bcc \(\beta'\), disordering above \(456\,^\circ\mathrm{C}\) into ductile \(\beta\) for hot working.
  • ② Answering Q2: \(\mathrm{Al\text{–}Cu}\) Three-Step Age Hardening: Solubility plunges from \(5.65\%\text{ Cu}\) (\(548\,^\circ\mathrm{C}\)) to \(<0.1\%\) at \(25\,^\circ\mathrm{C}\). In \(\mathrm{Al\text{–}4.4\%Cu}\): \(530\,^\circ\mathrm{C}\) solutionize into \(\alpha\) \(\to\) water quench into a soft supersaturated solution \(\to\) \(160\,^\circ\mathrm{C}\) age to nucleate dense nano-\(\mathrm{GP}\to\theta''\to\theta'\) plates that pin dislocations.
  • ③ \(\mathrm{Ti\text{–}Al}\) Aerospace Alloys: \(\mathrm{Al}\) raises the transus (\(\alpha\)-stabilizer) while \(\mathrm{V,Mo}\) stabilize bcc \(\beta\); workhorse \(\mathrm{Ti\text{–}6Al\text{–}4V}\) balances \(\alpha+\beta\) strength/toughness, and ordered \(\gamma\text{-TiAl}\) powers lightweight low-pressure turbine blades.
Textbook § 8.10 · Cu–Zn, Al–Cu & Ti–Al Alloys (Fig. 8.25)
§ 8.11.1 · TERNARY DIAGRAMS: GIBBS TRIANGLE, CONSTANT-PRESSURE RULE f* = 4 − P & JIN'S DIFFUSION MULTIPLES

Three Perpendicular Altitudes Sum to \(1\); Isothermal Three-Phase Regions Form Tie-Triangles

\(\begin{gathered}\tfrac{1}{2}a(d_{\mathrm{A}}+d_{\mathrm{B}}+d_{\mathrm{C}})=\tfrac{1}{2}a\cdot 1\implies x_{\mathrm{A}}+x_{\mathrm{B}}+x_{\mathrm{C}}=1\\ f^*=3-P+1=\mathbf{4-P}\;\;(P=3\Rightarrow f^*=1,\;P=4\Rightarrow f^*=0)\end{gathered}\)
  • Three Four-Phase Invariants (\(f^*=0\)): ① Ternary eutectic \(L\to\alpha+\beta+\gamma\); ② Ternary peritectic \(L+\alpha+\beta\to\gamma\); ③ Quasi-peritectic transition \(L+\alpha\to\beta+\gamma\).
  • Isothermal Sections & Jin Zhanpeng's Diffusion-Triple Method: Horizontal slices show two-phase tie-line bundles and straight-sided tie-triangles (three phase compositions fixed at vertices); Jin Zhanpeng pioneered ternary diffusion triples + EPMA scanning to map an entire isothermal section from one specimen.
Textbook § 8.11.1 · Gibbs Triangle & Diffusion Multiples (Fig. 8.26)
§ 8.11.2 · LIQUIDUS PROJECTION, ALKEMADE SADDLE THEOREM & THREE-STEP SOLIDIFICATION

Alkemade Lines Cut Boundary Valleys at Saddle Maxima \(S\), Carving Compatibility Triangles

\(\begin{gathered}\text{3-step path }(x_0\in\gamma\text{ field inside }\triangle DBC):\\ (1)\;L\to\gamma\;(\text{away from }C)\to(2)\;L\to\beta+\gamma\\ \to(3)\;\text{invariant }E_2:\;L\to\beta+\gamma+\delta\end{gathered}\)
  • Alkemade's Twin Verdicts: Joining the compositions of two adjacent primary phases (e.g., compound \(D\) and pure \(C\)): ① cuts their boundary valley at its maximum-temperature saddle \(S\) (liquid flows downhill away from \(S\)); ② partitions the diagram into compatibility triangles that uniquely fix which ternary invariant \(E_i\) ends freezing.
Textbook § 8.11.2 · Liquidus Projection & Alkemade Theorem (Fig. 8.27)
§ 8.11.3 · ISOPLETH LEVER-RULE BAN & THE Fe–Cr–Ni SCHAEFFLER WELD CONSTITUTION MAP

Tie-Lines Exit Vertical Isopleths—Never Apply the Lever Rule. Predict Welds via \(\mathrm{Cr_{eq}}\text{–}\mathrm{Ni_{eq}}\)

\(\begin{gathered}\mathrm{Cr_{eq}}=\mathrm{Cr}+\mathrm{Mo}+1.5\mathrm{Si}+0.5\mathrm{Nb}\;\;(\alpha\text{-stab.})\\ \mathrm{Ni_{eq}}=\mathrm{Ni}+30\mathrm{C}+0.5\mathrm{Mn}\;(+20\mathrm{N},\;\gamma\text{-stab.})\end{gathered}\)
  • What Isopleths Show vs. Forbid: A vertical cut such as \(\mathrm{Fe\text{–}18Cr\text{–}Ni}\) maps cooling phase sequences (\(430\) ferritic \(\to\) duplex \(\to\) \(304/316\) austenitic), but because conjugate tie-lines pierce out of the section plane, applying the lever rule on an isopleth is strictly invalid.
  • Welding Compass (\(3\text{–}8\%\;\delta\)): Retaining \(3\text{–}8\%\) \(\delta\)-ferrite along the base–filler dilution line prevents both \(100\%\;\gamma\) hot cracking and high-\(\delta\) \(\sigma\)-phase embrittlement.
Textbook § 8.11.3 · Isopleths & Schaeffler Weld Map (Fig. 8.28)
03
PART THREE

CALPHAD, Ellingham Diagram & Chapter Synthesis

Move Gibbs common-tangent hyperplanes into supercomputers to design 10-element single-crystal superalloys—then plot \(\Delta G^\circ(T)\) lines on the Ellingham diagram to decode pyrometallurgy.
  1. CALPHAD method: Redlich–Kister polynomials, Inden magnetism & Lagrange multipliers15
  2. Ellingham diagram: negative-slope \(\mathrm{2C+O_2\to 2CO}\) carbothermic smelting & nomograph16
  3. Chapter 8 master synthesis: equilibrium driving forces launching Chapters 9–1117
§ 8.12 · THE CALPHAD METHOD: PARAMETERIZING G^φ FOR HIGH-DIMENSIONAL HYPERPLANE OPTIMIZATION

Redlich–Kister Polynomials + Inden Magnetism + Lagrange \(\lambda_i=\mu_i^\phi\) Power 10-Element Superalloys

\(\begin{gathered}G^\phi=\sum_i x_i G_i^{0,\phi}+RT\sum_i x_i\ln x_i+G_{\mathrm{excess}}^\phi+G_{\mathrm{mag}}^\phi\\ G_{\mathrm{excess}}^\phi=\sum_i\sum_{j>i}x_i x_j\sum_\nu L_{ij}^{(\nu,\phi)}(x_i-x_j)^\nu\;\;(\nu=0:\;\text{reg.})\\ \min\sum_\phi f^\phi G^\phi\;\;\text{s.t.}\;\sum_\phi f^\phi x_i^\phi=x_i^0\implies\mu_i^\phi=\lambda_i\end{gathered}\)
  • “Binary Backbone + Ternary Refinement” Extrapolation: Pioneered by Kaufman & Hillert—calorimetry, activity, DFT, and Jin's diffusion multiples fit binary/ternary \(L_{ij}^{(\nu)}(T)\) plus Inden \(\mathrm{Fe/Co/Ni}\) magnetic terms to extrapolate reliably into \(10+\) component space.
  • Single-Crystal Superalloy “Compute First, Melt Second”: Across \(\mathrm{Ni,Cr,Co,W,Al,Ti,Ta,Re}\), CALPHAD pinpoints the \(\gamma'(\mathrm{Ni_3Al})\) solution window, avoids brittle TCP phases, and predicts Scheil solidification paths.
Fig. 8.29: CALPHAD Loop — Experiments / DFT → G^φ Database → Gibbs Minimization ① Expt. & DFT Inputs · Calorimetry ΔH / ai · Phase bounds / triples · DFT metastable E0 ② G^φ Database G⁰ + RTΣx ln x + Redlich–Kister Lij + Sublattice + Inden Gm ③ Gibbs Minimizer min Σ f^φ G^φ μi^α = μi^β = λi (Thermo-Calc / Pandat) Multicomp. Isopleths Solution heat-treat window Phase Fraction vs. T γ′ volume & TCP avoidance Scheil & Driving Force Feeds phase-field kinetics
Textbook § 8.12 · CALPHAD & Redlich–Kister Models (Fig. 8.29)
§ 8.13 · THE ELLINGHAM DIAGRAM: OXIDE STABILITY RANKINGS & CARBOTHERMIC REDUCTION

Metal Oxidation Lines Slope Upward (\(\Delta S^\circ\lt 0\)), While \(2\mathrm{C}+\mathrm{O_2}\to 2\mathrm{CO}\) Slopes Downward

\(\begin{gathered}\Delta G^\circ(T)=\Delta H^\circ-T\Delta S^\circ\;\;(\text{per }1\text{ mol }\mathrm{O_2})\\ \text{Slope}=-\Delta S^\circ:\;\;2\mathrm{M}+\mathrm{O_2}\to 2\mathrm{MO}\;(\gt 0)\\ 2\mathrm{C}+\mathrm{O_2}\to 2\mathrm{CO}\;(\Delta S^\circ\gt 0\Rightarrow\text{slope }\lt 0!)\end{gathered}\)
  • Lower Lines Reduce Upper Lines: Deep \(\mathrm{Al_2O_3}\) drives thermite welding of \(\mathrm{Fe_2O_3}\) and protective \(\mathrm{Al/Cr/Si}\) passive scales, whereas high \(\mathrm{Cu_2O}\) (decomposing above \(\sim 1900\,^\circ\mathrm{C}\)) let Bronze-Age smelters win copper in modest charcoal fires.
  • Answering Q3 (Coke Smelting vs. Kroll \(\mathrm{Ti}\)): The downward \(\mathrm{C\to CO}\) line cuts below \(\mathrm{FeO}\) (\(\sim 712\,^\circ\mathrm{C}\), blast furnace) and \(\mathrm{SiO_2}\) (\(\sim 1680\,^\circ\mathrm{C}\), submerged-arc \(\mathrm{Si}\)); \(\mathrm{Ti}\) forms brittle \(\mathrm{TiC}\) with carbon, requiring \(\mathrm{Mg}\) reduction of \(\mathrm{TiCl_4}\) (Kroll process).
Textbook § 8.13 · Ellingham Diagram & Smelting (Fig. 8.30)
CHAPTER 8 MASTER SYNTHESIS · FROM EQUILIBRIUM DESTINATION MAPS TO KINETIC EVOLUTION

Phase Diagrams Set Destination & Driving Force; Interfaces, Freezing & Transformations Set the Path

System TierCore Equilibrium MachineryEngineering Criteria & Signature Applications
Unary (\(C=1\))\(\mu^\alpha=\mu^\beta\implies\mathrm{d}p/\mathrm{d}T=\Delta H/(T\Delta V)\)Negative ice melting slope (\(-13.5\text{ MPa/K}\)), water triple point, supercritical \(\mathrm{CO_2}\) extraction
Binary Basics (\(C=2\))Common tangent + opposite-arm lever + \(f^*=3-P\)Miscibility gaps (\(475\,^\circ\mathrm{C}\) embrittlement), van 't Hoff slopes & dendritic coring segregation
Binary 3-PhaseThree-curve common tangent \(f^*=0\) (V vs. inverted-V)\(\mathrm{Pb\text{–}Sn}\) solders, \(\mathrm{Al\text{–}Si}\) modification, \(\mathrm{Cu\text{–}Pb}\) bearings, peritectic \(\sqrt{Dt}\) enveloping
Fe–C & Cu/Al/Ti\(1495/1148/727\,^\circ\mathrm{C}\) invariants + metastable tangentPearlite, cementite spheroidizing, ductile iron, \(\mathrm{Al\text{–}Cu}\) aging, \(\mathrm{Ti\text{–}6Al\text{–}4V}\) & \(\gamma\text{-TiAl}\)
Ternary & Comput.Gibbs triangle \(f^*=4-P\) · CALPHAD · EllinghamAlkemade paths, Schaeffler weld map, single-crystal superalloys, blast-furnace \(\mathrm{Fe}\) & \(\mathrm{Si}\)
Bridge Forward: Does cooling eutectoid steel below \(727\,^\circ\mathrm{C}\) always produce pearlite? No! Phase diagrams map equilibrium endpoints only—water quenching traps metastable martensite. Every boundary crosses an interface (Ch. 9), dropping below the liquidus triggers solidification (Ch. 10), and undercooling solids drives solid-state phase transformations (Ch. 11).
Textbook Ch. 8 Synthesis · Driving Force × Pathway × Rate
SUMMARY

Mastering Fe–C & Cu/Al/Ti Diagrams, Ternary Gibbs Space, CALPHAD & Pyrometallurgy

Fe–C Invariants & Pearlite→Metastable Tangent & Cast Irons→Cu–Zn · Al–Cu · Ti–Al→Gibbs Triangle & Schaeffler→CALPHAD & Ellingham
ANSWERING QUESTIONS 01 & 02

Hypereutectoid \(1.2\%\text{ C}\) steel precipitates only \(7.3\%\) secondary \(\mathrm{Fe_3C}\), yet it forms a continuous brittle network along prior-\(\gamma\) boundaries that requires spheroidizing annealing; water-quenching \(\mathrm{Al\text{–}4.4\%Cu}\) freezes a soft supersaturated \(\alpha\) solution so \(160\,^\circ\mathrm{C}\) aging can nucleate dense nano-\(\mathrm{GP/\theta''/\theta'}\) plates for peak strength.

ANSWERING QUESTION 03

Because \(2\mathrm{C}+\mathrm{O_2}\to 2\mathrm{CO}\) doubles gas moles (\(\Delta S^\circ\gt 0\)), its Ellingham line uniquely slopes downward, cutting below \(\mathrm{FeO}\) and \(\mathrm{SiO_2}\) at high \(T\) for carbothermic smelting; \(\mathrm{Ti}\) reacts with carbon to form \(\mathrm{TiC}\), requiring the \(\mathrm{Mg}\)-reduced \(\mathrm{TiCl_4}\) Kroll process.

Next up — Chapter 9 · Interfaces & Interfacial Energy: Gibbs adsorption, Young wetting, low-angle & CSL grain boundaries, Wulff shapes, and powder sintering.

Phase Equilibria & Phase Diagrams III · End of Chapter 8
CONCEPT QUIZ

Three Quick Questions: Click to Check or Launch a Live Class Poll

1. When eutectoid steel (\(0.77\%\text{ C}\)) transforms to equilibrium pearlite just below \(727\,^\circ\mathrm{C}\) (\(w_{\mathrm{C}}^\alpha=0.0218\%\), \(w_{\mathrm{C}}^{\mathrm{Fe_3C}}=6.69\%\)), what is the ferrite mass fraction, and how does metastable solubility compare with stable?

\(f^\alpha=(6.69-0.77)/(6.69-0.0218)\approx 88.8\%\); higher \(G^{\beta'}\) shifts the matrix tangent solute-rich (\(2.11\%\gt 2.08\%\)), so metastable solubility always exceeds stable solubility.

2. A point inside a unit-altitude Gibbs triangle has perpendicular distances \(0.3,0.5,0.2\) to sides \(BC,CA,AB\). What is \((x_{\mathrm{A}},x_{\mathrm{B}},x_{\mathrm{C}})\), and which rule holds for a ternary vertical isopleth?

Opposite-side altitudes give \((0.3,0.5,0.2)\); constant-\(p\) \(f^*=4-P\) allows up to 4 phases, and out-of-plane tie-lines forbid applying the lever rule on an isopleth.

3. Per mole of \(\mathrm{O_2}\): \(\mathrm{Si+O_2\to SiO_2}\) has \(\Delta H^\circ=-907.1\text{ kJ}\), \(\Delta S^\circ=-175\text{ J/K}\); \(2\mathrm{C+O_2\to 2CO}\) has \(\Delta H^\circ=-223.4\text{ kJ}\), \(\Delta S^\circ=+175.3\text{ J/K}\). Above what minimum temperature does carbon reduce \(\mathrm{SiO_2}\)?

Equating \(\Delta G^\circ\) gives \(T^*=(907\,100-223\,400)/(175+175.3)\) \(\approx 1952\text{ K}\) (\(1679\,^\circ\mathrm{C}\)), above which the negative-slope \(\mathrm{CO}\) line drops below \(\mathrm{SiO_2}\).

Phase Equilibria & Phase Diagrams III
FUNDAMENTALS OF MATERIALS SCIENCE · CHAPTER 8 COMPLETE

Thank You

6 Embedded Models: Iron–Carbon Phase Diagram · Eutectoid & Pearlite · Ternary Eutectic · 3D Ternary Liquidus Projection · Schaeffler Diagram · Ellingham Diagram — mse3d.com